Low-melting-point glass powder for matching MLCC (multilayer ceramic capacitor) I-type ceramic, conductive copper paste and multilayer ceramic capacitor

By adding TeO2 and Bi2O3 to the glass powder, the mass ratio is adjusted, the sintering temperature of MLCC Class I porcelain is reduced, the problems of leakage ceramics and ceramic body cracking are solved, and the quality and sintering density of MLCC components are improved.

CN118954956APending Publication Date: 2024-11-15SUZHOU GINET NEW MATERIAL TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411014974.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing glass powder used in MLCC Class I porcelain has high sintering temperature, resulting in problems such as leakage porcelain, excessive sagging distance after end sintering, and cracking of the ceramic body, and poor sintering density.

Method used

Boron-zinc-silicon glass powder is used as the basic component, TeO2 and Bi2O3 are added, and its mass ratio is adjusted, the sintering temperature is reduced to below 650°C, and the wetting and reactivity of the ceramic body are improved, so as to avoid leakage of ceramics and cracking.

Benefits of technology

Sintering at lower temperatures is achieved, the quality of MLCC components is improved, the problems of leakage ceramics and ceramic bodies are solved, and the adhesion and density after sintering are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954956A_ABST
    Figure CN118954956A_ABST
Patent Text Reader

Abstract

The invention discloses low-melting-point glass powder for matching MLCC (multilayer ceramic capacitor) I-type ceramic, conductive copper paste and a multilayer ceramic capacitor. The low-melting-point glass powder for matching the MLCC I-type porcelain, provided by the invention, is prepared from the following raw materials: a basic component and an improved component, wherein the basic component is boron-zinc-silicon glass, the improvement component contains TeO2 and Bi2O3, and the mass ratio of the basic component to TeO2 to Bi2O3 is 100: (0.1-5): (0.5-15); by adjusting the composition of the glass powder, the problem of ceramic leakage after sintering is solved, and meanwhile, the sintering temperature can be reduced to 650 DEG C or below, and the lowest sintering temperature can reach 600 DEG C; the thickness of the reaction layer can be controlled through low-temperature sintering, the problems of ceramic body cracking and overlong side sagging distance are solved, and the use performance of the multilayer ceramic capacitor is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of capacitors, and in particular to a low-melting-point glass powder, a conductive copper paste and a multilayer ceramic capacitor for matching MLCC type I porcelain. Background Art

[0002] MLCC (Multilayer Ceramic Capacitor) is known as the "rice of the electronics industry". Almost all electronic products require MLCC products. MLCC is composed of multiple thin ceramic sheets and electrodes. In the industry, MLCC can be divided into NPO, COG, Y5V, Z5U, X7R, X5R and other types according to temperature characteristics, materials, production processes, and filling media. Due to the different dielectric materials, the main polarization types are different, and the response speed and polarization rate to electric field changes are also different. The capacity is different under the same volume, and the dielectric loss and capacity stability of the capacitor are also different. Dielectric materials can be divided into two categories according to the temperature stability of capacity, namely Class I ceramic capacitors and Class II ceramic capacitors. Class I ceramic capacitors have excellent properties such as low dielectric loss, high insulation resistance, and linear change of dielectric constant with temperature.

[0003] Patent CN116535097A discloses a glass powder for MLCC. The glass powder can effectively avoid the damage caused by acidic conditions during electroplating, and the copper terminal electrode after slurry preparation has the advantages of excellent acid resistance, low porosity and high sintering densification. However, its sintering temperature is 750℃, which is relatively high. According to the data analysis provided by it, the sintered top morphology is poor, and the side hanging distance after the end slurry is sintered is too long, resulting in poor slurry density at the edges and porcelain leakage at the chamfers. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a low-melting-point glass powder, conductive copper paste and multilayer ceramic capacitor for matching MLCC Class I porcelain.

[0005] The present invention solves the technical problem by adopting the following technical solutions.

[0006] The present invention provides a low-melting-point glass powder for matching MLCC type I porcelain. The raw materials for making the low-melting-point glass powder include: a basic component and an improved component. The basic component is boron zinc silicon glass, the improved component contains TeO2 and Bi2O3, and the mass ratio of the basic component to TeO2 and Bi2O3 is 100:(0.1-5):(0.5-15). By adjusting the composition of the glass powder, the problem of porcelain leakage after sintering is solved, and the sintering temperature can be reduced to below 650°C, and the lowest temperature can reach 600°C. The problem of ceramic cracking can be improved by low-temperature sintering, and the problem of excessive side hanging distance can be solved.

[0007] The present invention also provides a conductive copper paste for MLCC. The raw materials of the conductive copper paste for MLCC include: the above-mentioned low-melting-point glass powder for matching MLCC Class I porcelain.

[0008] The present invention also provides a multilayer ceramic capacitor, which includes: a ceramic body and copper terminal electrodes, and the copper terminal electrodes are obtained by applying the above-mentioned conductive copper paste used for MLCC to both ends of the ceramic body by dipping and then performing end sintering treatment.

[0009] The present invention has the following beneficial effects:

[0010] The present invention provides a low-melting-point glass powder, a conductive copper paste and a multilayer ceramic capacitor for matching MLCC Class I porcelain. The present invention provides a glass powder with good compatibility with MLCC Class I porcelain and a low melting point. The low-melting-point glass powder uses boron zinc silicon glass as a basic component and is matched with an improved component. The low-melting-point glass powder of the above composition has good matching with the firing end temperature and the wettability of the ceramic body, so that the MLCC components can be fired at a lower temperature, and after the firing end, the components do not have a reaction layer that is too thick or a sag distance that is too long, or a porcelain leakage phenomenon, and have good sintering performance, thereby improving the quality of the MLCC components. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0012] Figure 1 This is a SEM image of the copper terminal electrode surface obtained by coating and sintering the conductive copper paste prepared by the low-melting-point glass powder provided in Examples 1 to 3;

[0013] Figure 2 The cross-sectional SEM image of the copper terminal electrode obtained by coating and sintering the conductive copper paste prepared by the low-melting-point glass powder provided in Examples 1 to 3;

[0014] Figure 3 The SEM image of the copper terminal electrode surface obtained by coating and sintering the conductive copper paste prepared by the low-melting-point glass powder provided in Comparative Examples 1 to 4;

[0015] Figure 4 The following are surface and cross-sectional SEM images of copper terminal electrodes obtained by coating and sintering a conductive copper paste prepared using the low-melting-point glass powder provided in Example 1. (1) and (2) are surface SEM images, and (3) and (4) are cross-sectional SEM images. DETAILED DESCRIPTION

[0016] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0017] The following is a detailed description of a low-melting-point glass powder, a conductive copper paste and a multilayer ceramic capacitor for matching MLCC Class I ceramics provided in an embodiment of the present invention.

[0018] In the first aspect, an embodiment of the present invention provides a low-melting-point glass powder for matching MLCC Class I porcelain, and its manufacturing raw materials include: a basic component and an improved component; wherein the basic component is boron zinc silicon glass, and the improved component contains TeO2 and Bi2O3, and the mass ratio of the basic component to TeO2 and Bi2O3 is 100:(0.1-5):(0.5-15); by adjusting the composition of the glass powder, the problem of porcelain leakage after sintering is solved, and at the same time, the sintering temperature can be reduced to below 650°C, and the lowest can reach 600°C; low-temperature sintering can improve the problem of ceramic cracking and solve the problem of sag length after glass melting.

[0019] MLCC electrodes are divided into inner electrodes and outer electrodes. The outer electrodes are used to connect the external circuit to the inner electrodes of MLCC. The outer electrode slurry is mainly composed of an organic phase, a bonding phase, and a conductive metal phase. The bonding phase is glass powder. With the development of MLCC, small size and high capacity are increasingly becoming the industry's pursuit of standards. This puts forward requirements for the firing end temperature and slurry matching of the outer electrode. If the firing end temperature is too high, on the one hand, it will lead to process waste. On the other hand, if the end-capping sintering temperature is too high, the reaction layer between the outer electrode and the MLCC ceramic body will be too thick, resulting in a decrease in subsequent reliability. This requires the softening point and melting point of the glass powder to develop towards a lower temperature. At a higher firing end temperature, the MLCC ceramic body is prone to expose defects in the ceramic body, such as cracking. In addition, there is a matching problem between the glass powder and the ceramic body. Some glass powders react violently with the ceramic body during the end-capping process, resulting in an overly thick reaction layer and ceramic body fragmentation. On the other hand, the glass powder has poor matching with the firing end temperature and the wettability of the ceramic body, resulting in too long side casting of the end slurry sintering and porcelain leakage on the top.

[0020] In order to solve the problem of porcelain leakage during end-capping sintering, an embodiment of the present invention provides a low-melting-point glass powder for matching MLCC Class I porcelain, and its raw materials include: a basic component and an improved component; wherein the basic component is boron zinc silicon glass, and the improved component contains TeO2 and Bi2O3, so that the conductive copper paste containing the low-melting-point glass powder can be fired at a temperature as low as 600°C during the preparation of the MLCC terminal electrode. The basic component of the low-melting-point glass powder is boron zinc silicon glass, which is widely used in the preparation of the bonding phase of the MLCC copper end paste due to its good processability and high-temperature fluidity, so the present invention selects this formula as the main skeleton. However, pure boron zinc silicon glass powder as a bonding phase has poor sintering density, wettability and acid resistance, and a high melting temperature. The low melting point glass powder prepared by the present invention is mainly boron zinc silicon glass, doped with TeO2 and Bi2O3 components, and improves the porcelain leakage problem existing in the above-mentioned prior art through the synergistic restraint of the two components; TeO2 has a significant effect of reducing the softening point and sintering temperature, and Bi2O3 reacts with the MLCC ceramic body, which can effectively control the flowability of the glass powder to improve the porcelain leakage problem of the end-capping slurry. However, excessive Bi2O3 will also cause the reaction layer between the glass powder and the ceramic body to be too thick, destroy the density of the ceramic body, and affect the performance in the later stage; but lowering the sintering temperature can improve the thickness of the reaction layer between Bi2O3 and the ceramic body, so by controlling the appropriate ratio of TeO2 and Bi2O3, while improving the porcelain leakage phenomenon, the thickness of the reaction layer is controlled to achieve the synergistic addition effect of the two components.

[0021] In an optional embodiment, the mass ratio of the basic component to TeO2 and Bi2O3 is 100:(0.1-5):(0.5-15). By controlling the mass ratio of the basic component to TeO2 and Bi2O3 in the glass powder, the problem of ceramic leakage after sintering can be solved, and the sintering end temperature of the external electrode can be reduced to below 650°C, and the lowest temperature can reach 600°C. Low-temperature sintering can improve the problem of ceramic cracking and solve the problem of sag length after glass melting.

[0022] Illustratively, the mass ratio of the base component to TeO2, Bi2O3 can be 100:0.1:0.5, 100:1:3, 100:1.5:4.5, 100:2.5:5.5, 100:3.0:5.0, 100:3.0:8.0, 100:3.5:6.5, 100:4.0:9.5, 100:4.0:10.0, 100:4.0:11.0, 100:4.5:13.0, 100:5.0:15.0 and any other value between 100:(0.1-5):(0.5-15).

[0023] In an optional embodiment, the amount of TeO2 used is 2.5%-5% of the total mass of the basic component, preferably 3.5%-5%; the amount of Bi2O3 used is 7.5%-15% of the total mass of the basic component, preferably 7.5%-10%.

[0024] Exemplarily, the percentage of TeO2 used in the total mass of the basic component can be 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0% and any other value between 2.5% and 5%; the percentage of Bi2O3 used in the total mass of the basic component can be 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, 10.0%, 10.5%, 11.0%, 11.5%, 12.0%, 12.5%, 13.0%, 13.5%, 14.0%, 14.5%, 15.0% and any other value between 7.5% and 15%.

[0025] In an optional embodiment, the mass ratio of Bi2O3 to TeO2 is (1.5:1)-(3.5:1). If the mass ratio of Bi2O3 to TeO2 is higher than 3.5:1, the adhesion of the end slurry after sintering is poor. If the mass ratio of Bi2O3 to TeO2 is lower than 1.5:1, the sintering temperature increases and the sintering adhesion is poor. Therefore, controlling the mass ratio of Bi2O3 to TeO2 to (1.5:1)-(3.5:1) can reduce the melting temperature of the glass powder, thereby reducing the end slurry sintering temperature to below 650°C, and the lowest can reach 600°C. Due to the low sintering temperature, the shrinkage rate of the copper end electrode slurry is small, the reactivity with the ceramic is moderate, and there is no cracking of the ceramic body.

[0026] Exemplarily, the mass ratio of Bi2O3 to TeO2 can be 1.5:1, 2.0:1, 2.5:1, 3.0:1, 3.5:1, and any other value between (1.5:1)-(3.5:1).

[0027] In an optional embodiment, the base component is composed of the following components in terms of mass percentage of oxides: B2O3: 30wt%-60wt%, ZnO: 10wt%-40wt%, SiO2: 1%-20%, TiO2: 0.1%-5%, BaO: 1%-8%; the total components are 100%.

[0028] Exemplarily, the base components are composed of the following components in terms of mass percentage of oxides: B2O3: 57wt%, ZnO: 40wt%, SiO2: 1%, TiO2: 1%, BaO: 1%, B2O3: 50wt%, ZnO: 40wt%, SiO2: 2%, TiO2: 3%, BaO: 5%, B2O3: 55wt%, ZnO: 25wt%, SiO2: 15.5%, TiO2: 0.5%, BaO: 4%, B2O3: 50wt%, ZnO: 30wt%, SiO2: 10%, TiO2: 2%, BaO: 8%, B2O3: 60wt%, ZnO: 20wt%, SiO2: 10%, TiO2: 4%, BaO: 6%, etc.

[0029] It is worth noting that the method for preparing the low-melting-point glass powder for matching MLCC Class I porcelain provided in the embodiment of the present invention comprises: mixing and sintering the raw materials of the basic component and the improved component in proportion, and then cooling and grinding to obtain the glass powder. That is, the glass powder can be prepared by the commonly used preparation method in the art.

[0030] In a second aspect, an embodiment of the present invention provides a conductive copper paste for MLCC, and the raw materials of the conductive copper paste for MLCC include: the above-mentioned low-melting-point glass powder for matching MLCC Class I porcelain.

[0031] In an optional embodiment, the raw materials of the conductive copper paste for MLCC include: copper powder, an organic carrier and the low-melting-point glass powder for matching MLCC Class I porcelain.

[0032] In an optional embodiment, the raw materials include the following components in percentage by mass: organic carrier: 14%-25%, copper powder: 65%-85%, glass powder: 3.5%-8%.

[0033] Exemplarily, the conductive copper paste includes the following components in percentage by mass: organic vehicle: 25%, copper powder: 70%, glass powder: 5%, organic vehicle: 20%, copper powder: 72%, glass powder: 8%, organic vehicle: 18%, copper powder: 74%, glass powder: 8%, etc.

[0034] In a third aspect, an embodiment of the present invention provides a multilayer ceramic capacitor, which includes: a Class I ceramic body and copper end electrodes, and the copper end electrodes are obtained by applying the above-mentioned conductive copper paste for MLCC to both ends of the Class I ceramic body and then subjecting it to a sintering end treatment.

[0035] In an optional embodiment, after the end-firing treatment at 600-700° C., the device has no porcelain leakage or cracking, and has a suitable sag distance and good adhesion.

[0036] Exemplarily, the burning end temperature can be 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, 700°C and any other value between 600 and 700°C.

[0037] As can be seen from the above, the embodiments of the present invention provide a low-melting-point glass powder, conductive copper paste and multilayer ceramic capacitor for matching MLCC Class I porcelain. The low-melting-point glass powder for matching MLCC Class I porcelain provided in the embodiments of the present invention comprises: a basic component and an improved component; wherein the basic component is boron zinc silicon glass, and the improved component contains TeO2 and Bi2O3, so that the conductive copper paste containing the low-melting-point glass powder has a sintering temperature as low as 600°C during the preparation of the MLCC terminal electrode. The use of the conductive copper paste containing the above-mentioned low-melting-point glass powder can solve the current problems of too long sag on the side of the terminal paste and ceramic leakage at the edges and corners. At the same time, by adjusting the glass powder component, the sintering temperature can be reduced to 600°C, and low-temperature sintering in the range of 600-700°C can be achieved. Moreover, because the sintering temperature is low, the shrinkage rate of the copper terminal electrode slurry is small, the reactivity with Class I ceramics is moderate, and there is no cracking of the Class I ceramic body.

[0038] The present invention will be further described below in conjunction with the embodiments.

[0039] Example 1

[0040] The following components B2O3:ZnO:SiO2:TiO2:BaO=55:25:15.5:0.5:4 are weighed as the basic components of the glass powder and ground evenly, and then the improved components TeO2 and Bi2O3 are weighed and ground evenly according to the mass ratio of the basic components to the improved components TeO2 and Bi2O3 of 100:3:5;

[0041] The solid powder with improved components added and ground evenly is placed in a crucible at 1000°C and kept warm for 1.5 hours to be sintered into glass liquid.

[0042] Pour the glass liquid into cold water for quenching, and crush it after cooling.

[0043] The glass particles are ground evenly to obtain glass powder.

[0044] The glass powder, copper powder and organic carrier are uniformly mixed to prepare a slurry.

[0045] The slurry is coated on the end of the Class I ceramic body by dipping, and then sintered to prepare a copper terminal electrode at a sintering temperature of 600°C.

[0046] Example 2

[0047] The following components B2O3:ZnO:SiO2:TiO2:BaO=50:30:10:2:8 are weighed as the basic components of the glass powder and ground evenly, and then the improved components TeO2 and Bi2O3 are weighed and ground evenly according to the mass ratio of the basic components to the improved components TeO2 and Bi2O3 of 100:5:8;

[0048] The solid powder with improved components added and ground evenly is placed in a crucible at 1000°C and kept warm for 1.5 hours to be sintered into glass liquid.

[0049] Pour the glass liquid into cold water for quenching, and crush it after cooling.

[0050] The glass particles are ground evenly to obtain glass powder.

[0051] The glass powder, copper powder and organic carrier are uniformly mixed to prepare a slurry.

[0052] The slurry is coated on the end of the Class I ceramic body by dipping, and then sintered to prepare a copper terminal electrode at a sintering temperature of 600°C.

[0053] Example 3

[0054] The following components B2O3:ZnO:SiO2:TiO2:BaO=60:20:10:4:6 are weighed as the basic components of the glass powder and ground evenly, and then the improved components TeO2 and Bi2O3 are weighed and ground evenly according to the mass ratio of the basic components to the improved components TeO2 and Bi2O3 of 100:3:8;

[0055] The solid powder with improved components added and ground evenly is placed in a crucible at 1000°C and kept warm for 1.5 hours to be sintered into glass liquid.

[0056] Pour the glass liquid into cold water for quenching, and crush it after cooling.

[0057] The glass particles are ground evenly to obtain glass powder.

[0058] The glass powder, copper powder and organic carrier are uniformly mixed to prepare a slurry.

[0059] The slurry is coated on the end of the Class I ceramic body by dipping, and then sintered to prepare a copper terminal electrode at a sintering temperature of 600°C.

[0060] Comparative Example 1

[0061] Compared with Example 1, the only difference is that the mass ratio of the basic component to the improved components TeO2 and Bi2O3 is 100:5:0.

[0062] Comparative Example 2

[0063] Compared with Example 1, the only difference is that the mass ratio of the basic component to the improved components TeO2 and Bi2O3 is 100:5:5.

[0064] Comparative Example 3

[0065] Compared with Example 1, the only difference is that the mass ratio of the basic component to the improved components TeO2 and Bi2O3 is 100:4:15.

[0066] Comparative Example 4

[0067] Compared with Example 1, the only difference is that the mass ratio of the basic component to the improved components Sb2O3 and Bi2O3 is 100:3:5:.

[0068] Test Results

[0069] Figure 1 The surface SEM images of the copper terminal electrodes obtained by coating and sintering the conductive copper paste prepared by the low melting point glass powder provided in Examples 1 to 3 are shown in FIG. Figure 1 It can be seen that the top surfaces of the copper terminal electrodes provided in Examples 1 to 3 are sintered densely without any porcelain leakage or holes.

[0070] Figure 2 The SEM image of the cross section of the copper terminal electrode obtained by coating and sintering the conductive copper paste prepared by the low melting point glass powder provided in Examples 1 to 3. Figure 2 It can be seen that the cross-section of each embodiment is sintered densely, the slurry wrapping at the chamfer is good, and the side sag distance is appropriate;

[0071] Figure 3 This is a SEM image of the copper terminal electrode surface obtained by coating and sintering the conductive copper paste prepared by the low-melting-point glass powder provided in Comparative Examples 1 to 4. Figure 3 Microscope analysis of Comparative Example 1 shows that when the only improved component is TeO2, the copper terminal electrode of Comparative Example 1 has poor adhesion after sintering; in Comparative Example 2, when Bi2O3:TeO2=1<1.5, the SEM image of the top surface of the sintered copper terminal electrode shows that there are many holes on the sintered surface, and porcelain leakage occurs at the chamfers; in Comparative Example 3, when Bi2O3:TeO2=3.75>3.5, the SEM image of the sintered cross-section of the copper terminal electrode shows obvious porcelain body fragmentation at the contact between the copper terminal electrode and the ceramic body; in Comparative Example 4, after TeO2 is replaced with Sb2O3, it can be seen from the SEM image of the sintered surface of the copper terminal electrode that there are many holes on the sintered surface and it is not dense.

[0072] Figure 4 The surface and cross-section SEM images of the copper terminal electrode obtained by coating and sintering the conductive copper paste prepared by the low-melting-point glass powder provided in Example 1 are shown in FIG. Figure 4The surface SEM images of (1) and (2) show that the surface of the copper terminal electrode in Example 1 is sintered densely, with no porcelain leakage at the chamfered corners and no holes. Figure 4 From the cross-sectional SEM images of (3) and (4), it can be seen that the cross-sectional sintering of the copper terminal electrode is dense, the slurry wrapping at the chamfer is good, and the side sag distance is appropriate.

[0073] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A low melting point glass powder for matching MLCC Class I porcelain, characterized in that: The raw materials for its production include: a basic component and an improved component; wherein the basic component is boron zinc silicon glass, the improved component contains TeO2 and Bi2O3, and the mass ratio of the basic component to TeO2 and Bi2O3 is 100:(0.1-5):(0.5-15); by adjusting the composition of the glass powder, the problem of porcelain leakage after sintering can be solved, and at the same time the sintering temperature can be reduced to below 650°C, and the lowest can reach 600°C; by low-temperature sintering, the problem of ceramic cracking can be improved, and the problem of long side sag after sintering of the copper end slurry can be solved.

2. The low-melting-point glass powder for matching MLCCI type porcelain according to claim 1, characterized in that: The mass ratio of the basic component to TeO2 and Bi2O3 is 100:(0.1-5):(0.5-15), wherein the proportion of TeO2 is preferably 2.5%-5%, more preferably 3.5%-5%, and the proportion of Bi2O3 is preferably 7.5%-15%, more preferably 7.5%-10%; at the same time, the ratio of Bi2O3 to TeO2 is controlled to be (1.5):1-(3.5:1); if it is higher than 3.5:1, the slurry adhesion after sintering is poor; if it is lower than 1.5:1, the sintering temperature increases and the sintering adhesion is poor.

3. The low-melting-point glass powder for matching MLCCI type porcelain according to claim 1, characterized in that: The basic components are composed of the following components in terms of mass percentage of oxides: B2O3: 30%-60%, ZnO: 10%-40%, SiO2: 1%-20%, TiO2: 0.1%-5%, BaO: 1%-8%; the total components are 100%.

4. The low-melting-point glass powder for matching MLCCI type porcelain according to claim 1, characterized in that: By adjusting the mass ratio of the basic component to TeO2 and Bi2O3, the wettability of the glass powder and the MLCCI type porcelain body can be improved, and the porcelain leakage phenomenon after sintering can be solved.

5. The low melting point glass powder for matching MLCCI type porcelain according to claim 1, characterized in that: By adjusting the mass ratio of the basic components to TeO2 and Bi2O3, the melting temperature of the glass powder can be reduced, thereby reducing the end slurry sintering temperature to below 650°C, and the lowest can reach 600°C; by lowering the sintering temperature, the end slurry stress and reactivity with the ceramic body are reduced, thereby avoiding cracking of the ceramic body.

6. A conductive copper paste for MLCC, characterized in that: The raw materials for the conductive copper paste for MLCC include: the low-melting-point glass powder for matching MLCC Class I porcelain according to any one of claims 1 to 5.

7. The conductive copper paste for MLCC Class I ceramic body according to claim 6, characterized in that: The raw materials of the conductive copper paste for MLCC include: copper powder, organic carrier and low-melting-point glass powder.

8. The conductive copper paste for MLCC Class I ceramic body according to claim 7, characterized in that: The raw materials include the following components in percentage by mass: organic carrier: 14%-25%, copper powder: 65%-85%, and glass powder: 3.5%-8%.

9. A multilayer ceramic capacitor, characterized in that: The multilayer ceramic capacitor comprises: a Class I ceramic body and copper terminal electrodes, and the copper terminal electrodes are obtained by applying the conductive copper paste for MLCC described in any one of claims 6 to 8 to both ends of the Class I ceramic body by dipping, and then subjecting the end to sintering treatment.

10. The multilayer ceramic capacitor according to claim 9, characterized in that: After sintering at 600-700℃, the device has no porcelain leakage or cracking, and has a suitable sag distance and good adhesion.

Citation Information

Patent Citations

  • Glass powder for MLCC (multilayer ceramic capacitor), conductive copper paste, multilayer ceramic capacitor and preparation method

    CN116535097A

  • Glass powder for crystalline silicon solar cell front silver paste and preparation method thereof

    CN105174728A

  • Glass powder for low-temperature sealing, preparation method and application

    CN109399944A

  • Glass powder for photovoltaic ink and preparation method thereof

    CN114249538A

  • 5G ceramic filter electrode silver paste with high adhesive force and preparation method thereof

    CN114709002A