High-transparency stable super-hydrophobic coating and preparation method thereof
Through the combination of high-temperature sintering technology and organosilane coupling agent, the problem of insufficient stability of transparent superhydrophobic coating is solved, and a superhydrophobic coating with high transparency and excellent antifouling performance is achieved. It is suitable for a variety of optical window materials.
Patent Information
- Application Number
- CN202411024355.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The existing transparent superhydrophobic coatings have problems with fragile coatings and insufficient stability, especially in the difficulty of optimal balance between optical transmittance and mechanical stability.
Using high-temperature treatment inorganic cross-linking technology, the nanosol is formed by stirring SiO2 nanoparticles in a dispersing solvent and sintering in a muffle furnace. The hydrolysis and condensation reaction is carried out in a vacuum drying chamber with organic silane coupling agent to enhance the nanometers. The bonding force between the particles and the substrate.
The stability and durability of the nanoparticle accumulation structure are significantly improved, while maintaining high transparency, avoiding significant reduction in optical transmittance, and achieving excellent anti-fouling and self-cleaning performance.
Smart Images

Figure CN118954964A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of super-hydrophobic materials, and in particular relates to a highly transparent and stable super-hydrophobic coating based on high-temperature treatment of inorganic cross-linking and a preparation method thereof. Background Art
[0002] The achievement of super-hydrophobic properties requires the construction of a unique micro-nanostructure. When the structure is applied to transparent window materials such as glass, it is necessary to ensure that its super-hydrophobic performance is fully utilized, and it is necessary to fully consider the optical properties of the material itself and the influence of the structure on light transmission, so as to ensure that transparency and super-hydrophobic performance reach the best balance. Specifically, in order to achieve super-hydrophobicity, it is necessary to perform a roughening process on the substrate surface. However, improving the surface roughness may have a significant impact on transparency and mechanical stability. When the surface roughness is too large, especially when it reaches a level sufficient to induce Mie scattering, a significant light scattering surface may be formed, thereby reducing the transparency of the material. Therefore, the mainstream solution for preparing transparent super-hydrophobic coatings currently uses nanoparticles with a size of less than 100nm. The self-similar structure formed by the accumulation of nanoparticles has excellent anti-infiltration characteristics, thereby effectively improving the weather resistance of the coating. However, the transparent super-hydrophobic surface coating formed by this nanoparticle accumulation structure has the defects of fragile coating and insufficient stability.
[0003] Improving the stability between nanoparticles and the bonding force between substrates has always been a difficult point of research. CN117701114A describes a method that achieves a transparent super-hydrophobic coating on a glass surface by mixing nano-SiO2 powder and ATO powder and spraying them on a glass surface. However, the experimental results show that the optical transmittance of the coating is reduced by about 20% compared to a blank sample, showing a significant light transmittance loss. A method for preparing a transparent super-hydrophobic coating described in CN116924698A is by embedding hydrophobic silica on a polyurethane layer surface to form. However, it is worth noting that due to the easy occurrence of delamination and shedding phenomenon with inorganic particles in the aging process of organic resins, this may have an adverse effect on the stability and durability of the coating. Summary of the Invention
[0004] The purpose of the present invention is to propose a highly transparent and stable super-hydrophobic coating based on high-temperature treatment of inorganic cross-linking and a preparation method thereof, so as to solve the technical problems of the existing coatings mentioned in the above background technology, such as the fragility and insufficient stability of the coating.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a highly transparent and stable super-hydrophobic coating based on high-temperature treatment of inorganic cross-linking, specifically comprising the following steps:
[0007] (1) SiO2 nanoparticles are added to a dispersion solvent to prepare a nanoparticle dispersion liquid, the nanoparticle dispersion liquid is stirred by a stirring device to prepare a uniform nanosol, a transparent substrate is immersed in the nanosol, and then the transparent substrate is pulled out and dried; or the nanosol is sprayed on the surface of the transparent substrate with a spray gun and then dried;
[0008] (2) placing the substrate coated with nanoparticles obtained in step (1) in a muffle furnace, gradually raising the temperature in the furnace to a sintering temperature according to a predetermined heating program, maintaining the temperature after reaching the sintering temperature, and then annealing the substrate in a furnace cooling manner;
[0009] (3) placing the substrate obtained in step (2) and the organic silane coupling agent together in a vacuum drying oven, setting the temperature and keeping the temperature.
[0010] Furthermore, in step (1), the nanoparticles are about 40 nm, the dispersion solvent is isopropyl alcohol, the concentration of the nanoparticle dispersion is about 5 wt‰, the stirring time is 6 hours, the stirring device is a digital stirrer or a ball milling device, and the immersion time is 10 minutes.
[0011] Furthermore, in step (2), the predetermined heating program refers to gradually increasing the temperature in the furnace to a sintering temperature of 700°C at a constant rate of 4°C per minute, and the holding time is 10 minutes.
[0012] Furthermore, in step (3), the amount of the organic silane coupling agent is 2 μl, the temperature is set to 60° C., and the insulation time is 2 h.
[0013] Furthermore, in step (1), the dispersion solvent is any one of organic solvents such as ethanol, propanol, isopropanol, acetone or ethyl acetate.
[0014] Furthermore, in step (3), the organosilane coupling agent includes a fluorine-containing organosilane coupling agent and a fluorine-free organosilane coupling agent; the fluorine-free organosilane coupling agent includes KH-550, KH-540, KH-902, and KH-554; the fluorine-containing organosilane coupling agent includes perfluorodecyltrichlorosilane, perfluorohexyltrichlorosilane, perfluorooctyltrichlorosilane, perfluorododecyltrichlorosilane, perfluorohexyltrimethoxysilane, perfluorooctyltrimethoxysilane, perfluorodecyltrimethoxysilane, perfluorohexyltriethoxysilane, perfluorooctyltriethoxysilane, and perfluorodecyltriethoxysilane.
[0015] Another object of the present invention is to provide a highly transparent and stable super-hydrophobic coating prepared by the above method.
[0016] The present invention has the following beneficial effects:
[0017] The present invention proposes an innovative solution, which is to improve the bonding force between particles and particles, as well as between particles and substrates in the nanoparticle stacking structure through high-temperature sintering technology. In this process, the nanoparticles are treated at high temperature, and the interaction and bonding force between the particles are significantly enhanced. The advantage of this method is that it can improve the stability and durability of the nanoparticle stacking structure to a certain extent without affecting the transparency. It is a purely inorganic particle bonding strategy that aims to use high-temperature sintering technology to tightly connect nanoparticles together to form a highly ordered and stable structure. Compared with traditional organic binders, pure inorganic particle bonding has the advantages of being not easy to age, high temperature resistant, and corrosion resistant. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0019] Figure 1 Schematic diagram for the preparation of nanoparticle stacking structure;
[0020] Figure 2 This is a scanning electron micrograph of the sample in the unsintered state;
[0021] Figure 3 This is a scanning electron micrograph of the sample sintered at 700°C;
[0022] Figure 4 This is a scanning electron micrograph of the sample sintered at 900°C;
[0023] Figure 5 This is a scanning electron micrograph of the sample sintered at 1000°C;
[0024] Figure 6 is the salt spray cycle test result;
[0025] Figure 7 The transmittance measurement result.
[0026] In the accompanying drawings, the symbols represent the following:
[0027] Nanoparticles-1, dispersion solvent-2, nanoparticle dispersion-3, stirring device-4, nanosol-5, transparent substrate-6, spray gun-7. DETAILED DESCRIPTION
[0028] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] See Figure 1-7 As shown, a method for preparing a highly transparent and stable super-hydrophobic coating based on high-temperature treatment of inorganic cross-linking specifically comprises the following steps:
[0031] Step 1: Preparation of nanoparticle stacking structure
[0032] Select SiO2 nanoparticles 1 of about 40nm, disperse them in a dispersion solvent 2, the dispersion solvent 2 is isopropyl alcohol, and prepare a nanoparticle dispersion 3 with a concentration of about 5wt‰; use a stirring device 4 to stir the nanoparticle dispersion 3 for 6 hours to make a uniform nanosol 5, the stirring device 4 is a digital display stirrer or a ball milling device; soak a transparent substrate 6 in the nanosol 5, soak for 10 minutes, then pull it out and dry it. The nanosol 5 can also be sprayed on the surface of the transparent substrate 6 using a spray gun 7, and different times can be sprayed without affecting the transparency. This step process is as follows Figure 1 shown.
[0033] The dispersion solvent 2 in this step is selected from any one of organic solvents such as ethanol, propanol, isopropanol, acetone or ethyl acetate.
[0034] Step 2: High temperature sintering
[0035] The substrate coated with nanoparticles obtained in step one is placed in a muffle furnace. According to a predetermined heating program, the temperature in the furnace is gradually increased to a sintering temperature of 700°C at a constant rate of 4°C per minute. After reaching the sintering temperature, the sintering temperature state is maintained for 10 minutes to ensure that the sintering process is fully carried out. Subsequently, the substrate is annealed as the temperature of the muffle furnace gradually decreases in a furnace cooling manner. After this treatment process is completed, the morphology of the particles on the surface of the substrate is observed using scanning electron microscopy (SEM) technology, and its characterization image is obtained, as shown in FIG. Figure 3 shown.
[0036] Step 3: Surface superhydrophobic modification
[0037] The present invention uses vapor deposition to hydrophobically modify the coating. The sample obtained in step 2 is placed in a vacuum drying oven along with 2 μl of an organosilane coupling agent, ensuring a strict vacuum environment. The temperature is then set to 60°C and maintained for 2 hours to promote a thorough reaction. This process successfully achieves hydrophobic modification of the coating particles by precisely controlling the hydrolysis-condensation reaction between the organosilane coupling agent and the nanoparticles, ensuring both accuracy and effectiveness of the modification.
[0038] The organosilane coupling agent in this step includes a fluorine-containing organosilane coupling agent and a fluorine-free organosilane coupling agent; the fluorine-free organosilane coupling agent includes KH-550, KH-540, KH-902, and KH-554; the fluorine-containing organosilane coupling agent is selected from perfluorodecyltrichlorosilane, perfluorohexyltrichlorosilane, perfluorooctyltrichlorosilane, perfluorododecyltrichlorosilane, perfluorohexyltrimethoxysilane, perfluorooctyltrimethoxysilane, perfluorodecyltrimethoxysilane, perfluorohexyltriethoxysilane, perfluorooctyltriethoxysilane, and perfluorodecyltriethoxysilane.
[0039] Example 2
[0040] The only difference from Example 1 is that the final sintering temperature in step 2 is 900°C. Figure 4 The electron micrographs at 900℃ sintering temperature are given.
[0041] Example 3
[0042] The only difference from Example 1 is that the final sintering temperature in step 2 is 1000°C. Figure 5 Electron microscopy images at a sintering temperature of 1000°C are given.
[0043] To compare the coating before and after sintering, Figure 2 Electron micrographs of the unsintered samples are shown. Comparative analysis of the images reveals that the surface particles of the samples sintered at high temperatures are more robust than those of the unsintered samples, with a higher packing density. However, when the sintering temperature is too high, reaching 1000°C, the surface particles become agglomerated, resulting in a decrease in surface roughness.
[0044] To determine the optimal sintering temperature, samples from Examples 1, 2, and 3 were subjected to a salt spray cycle test. During this process, the samples were exposed to a highly salt-fog atmosphere to simulate the real-world corrosion of the coating under the action of small fog droplets. High-salt fog environments have a significant corrosive effect on optical windows. The salt spray test simulates the corrosion of the coating in the presence of small fog droplets. This testing process strictly adheres to a 24-hour salt spray cycle followed by a 24-hour drying period to ensure the accuracy and reliability of the test results. Figure 6 The results of the salt spray cycle test are given.
[0045] Experimental verification shows that for samples sintered at a sintering temperature of 700°C, after two salt spray cycle tests, the contact angle showed a smaller downward trend, demonstrating a more stable weather resistance effect.
[0046] To ensure accurate assessment of surface transparency after sintering, the samples were tested for transmittance using a UV-visible spectrophotometer. During the test, a blank sample was set as the benchmark (its transmittance was defined as 100%), and the transmittance of the coating was measured accordingly.
[0047] Figure 7 The transmittance measurements are presented. Analysis of the data in the graph shows that the sintered samples exhibit excellent transmittance, approaching the standard for bare glass. More notably, within a specific wavelength range (600-800nm), the transmittance of the sintered samples exhibits an enhanced transmittance effect.
[0048] The present invention adopts an immersion and pulling method to prepare a nanoparticle stacking structure on a transparent substrate, which has good transparency; a high-temperature sintering process is used to improve the bonding between coating particles and between particles and the substrate; the structure combined with pure inorganic particles can prepare a super-hydrophobic structural material with excellent performance and stability. Compared with traditional organic binders, the pure inorganic particle bonding has the advantages of being not easy to age, high temperature resistant, and corrosion resistant.
[0049] The coating of this invention utilizes an all-inorganic structure and, through a high-temperature sintering process, forms a highly stable superhydrophobic surface, exhibiting excellent antifouling and self-cleaning properties. This coating is suitable for surfaces requiring high transparency, such as automotive glass, photovoltaic protective panels, architectural glass, and marine optical windows.
[0050] The preferred embodiments of the present invention disclosed above are intended only to help illustrate the present invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the present invention to the specific embodiments described. Obviously, numerous modifications and variations are possible based on the contents of this specification. These embodiments are selected and described in detail in this specification to better explain the principles and practical applications of the present invention, thereby enabling those skilled in the art to better understand and utilize the present invention.
Claims
1. A method for preparing a highly transparent and stable super hydrophobic coating based on high temperature treatment of inorganic cross-linking, characterized in that: The specific steps include: (1) adding SiO2 nanoparticles into a dispersion solvent to prepare a nanoparticle dispersion liquid, stirring the nanoparticle dispersion liquid with a stirring device to prepare a uniform nanosol, immersing a transparent substrate in the nanosol, and then pulling out the transparent substrate to dry; or spraying the nanosol on the surface of the transparent substrate with a spray gun and then drying; (2) placing the substrate coated with nanoparticles obtained in step (1) in a muffle furnace, gradually raising the temperature in the furnace to a sintering temperature according to a predetermined heating program, maintaining the temperature after reaching the sintering temperature, and then annealing the substrate in a furnace cooling manner; (3) placing the substrate obtained in step (2) and the organic silane coupling agent together in a vacuum drying oven, setting the temperature and keeping the temperature.
2. The method for preparing a highly transparent and stable super hydrophobic coating based on high temperature treatment of inorganic crosslinking according to claim 1, characterized in that: In step (1), the nanoparticles are about 40 nm, the dispersion solvent is isopropanol, the concentration of the nanoparticle dispersion is about 5 wt‰, and the stirring device is a digital stirrer or a ball mill.
3. The method for preparing a highly transparent and stable super hydrophobic coating based on high temperature treatment inorganic cross-linking according to claim 1, characterized in that: In step (2), the predetermined heating program refers to gradually increasing the temperature in the furnace to a sintering temperature of 700° C. at a constant rate of 4° C. per minute.
4. The method for preparing a highly transparent and stable super hydrophobic coating based on high temperature treatment of inorganic crosslinking according to claim 3, characterized in that: In step (3), the amount of the organic silane coupling agent is 2 μl, and the temperature is set to 60° C.
5. A method for preparing a highly transparent and stable super hydrophobic coating based on high temperature treatment inorganic cross-linking according to any one of claims 1 to 4, characterized in that, In step (1), the dispersing solvent is any one of organic solvents such as ethanol, propanol, isopropanol, acetone or ethyl acetate.
6. A method for preparing a highly transparent and stable super hydrophobic coating based on high temperature treatment of inorganic crosslinking according to any one of claims 1 to 4, characterized in that: In step (3), the organosilane coupling agent includes a fluorine-containing organosilane coupling agent and a fluorine-free organosilane coupling agent; the fluorine-free organosilane coupling agent includes KH-550, KH-540, KH-902, and KH-554; the fluorine-containing organosilane coupling agent includes perfluorodecyltrichlorosilane, perfluorohexyltrichlorosilane, perfluorooctyltrichlorosilane, perfluorododecyltrichlorosilane, perfluorohexyltrimethoxysilane, perfluorooctyltrimethoxysilane, perfluorodecyltrimethoxysilane, perfluorohexyltriethoxysilane, perfluorooctyltriethoxysilane, and perfluorodecyltriethoxysilane.
7. A highly transparent and stable super hydrophobic coating prepared by the preparation method according to any one of claims 1 to 6.
Citation Information
Patent Citations
Method for preparing transparent super-hydrophobic automatic cleaning coating
CN101519278A
Method for constructing transparent, super-hydrophobic and self-cleaning nano coating with low cost by taking soot as template
CN103553359A
Method for preparing superhydrophobic coating layer through composite of inorganic nano-particles with different average particle sizes
CN105602297A
Preparation method of transparent superhydrophobic coating
CN110669363A
Hydrophobic coating with strong adhesive force with substrate and preparation method thereof
CN114082617A
Cited By
Multi-scale constructed high-transparency stable super-hydrophobic coating and preparation method thereof
CN119608545A
A high-transparency stable super-hydrophobic coating constructed in multiple scales and a preparation method thereof
CN119608545B