Preparation method of cementing material
By mixing medical waste slag and fly ash with red mud and desulfurized gypsum to prepare cementitious materials, the problem of post-incineration treatment of medical waste has been solved, achieving harmless disposal and resource utilization, and reducing production costs.
Patent Information
- Application Number
- CN202411031931.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The disposal of slag and fly ash from medical waste incineration poses safety hazards and is difficult to utilize as resources. Traditional cement production also suffers from high energy consumption and high costs.
Medical waste slag, medical waste fly ash, red mud and desulfurized gypsum are mixed and then granulated and melt-sintered to produce slag-based cement. This cement is then mixed with silicate cement and cured to produce a cementitious material.
It achieves the harmless disposal of medical waste incineration slag and fly ash, reduces the heavy metal content, and the resulting cementitious material can replace traditional cement, reducing production costs and realizing resource utilization.
Smart Images

Figure CN118954986A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of industrial waste resource utilization, and in particular to a method for preparing a gelling material. Background Art
[0002] Medical waste is waste that is directly or indirectly infectious, toxic, or otherwise hazardous and is generated by medical institutions during medical treatment and related activities. Due to its inherently dangerous nature, the treatment of medical waste has attracted widespread attention. At present, high-temperature incineration is the main method for treating medical waste at home and abroad. It has the advantages of a wide range of applications, significant volume reduction, and thorough disinfection and sterilization. However, byproducts such as slag and fly ash generated during the incineration process contain harmful components such as heavy metals and soluble chloride salts. Therefore, it is also necessary to pay attention to the safety hazards brought by these byproducts.
[0003] At present, the disposal of medical waste incineration slag is mainly sanitary landfill after stabilization. However, with the increasing shortage of land resources, the sanitary landfill capacity is constantly decreasing, and the constraints of factors such as the difficulty in site selection for new landfills have made it difficult for incineration slag to be placed. At the same time, the main methods for treating fly ash include cement solidification and stabilization, chemical treatment, and safe landfill, but there are generally problems of high disposal costs and high technical difficulty.
[0004] Cementitious materials refer to materials that can bind loose or block materials into a whole through their own physical and chemical effects, in the process of changing from a plastic slurry to a hard stone-like body. Hydraulic cementitious materials can harden in both air and water after being slurried with water. This type of material is generally called cement, such as silicate cement. This type of cement requires a large amount of fuel to calcine the raw materials and sinter them into cement clinker during the production process, which not only consumes a lot of energy, but also releases a lot of carbon dioxide.
[0005] The slag and fly ash left after the incineration of medical waste contain the main ingredients for producing cement. Using the slag and fly ash left after the incineration of medical waste in cement production can not only solve the problem of medical waste disposal, but also reduce the use of traditional cement and reduce production costs.
[0006] Therefore, there is an urgent need to provide a method for preparing cementitious materials using medical waste slag and fly ash. Summary of the invention
[0007] In view of the above shortcomings of the prior art, the present invention provides a method for producing a cementitious material, which can achieve the harmless disposal of medical waste incineration slag and fly ash, and can convert high-temperature molten products into cementitious materials to achieve resource utilization of waste.
[0008] To achieve the above object and other related objects, the present invention provides a method for preparing a gelling material, which comprises the following steps:
[0009] Medical waste slag, medical waste fly ash, red mud, desulfurized gypsum and slag cooling water are mixed and stirred uniformly to prepare a mixed slurry;
[0010] The mixed slurry is granulated and then dried to obtain green body particles;
[0011] The green body particles are subjected to melting and sintering treatment, cooled, and then ground to obtain slag-based cement;
[0012] The slag-based cement is mixed with silicate cement and cured to obtain a cementitious material.
[0013] In one example of the present invention, the mass ratio of the medical waste slag, medical waste fly ash, red mud and desulfurization gypsum is (1-3): (1-5): (1-2): (1-3); the mass of the slag cooling water accounts for 1% to 10% of the total mass of the mixed slurry.
[0014] In one example of the present invention, the particle size of the medical waste slag, the medical waste fly ash, the red mud and the desulfurization gypsum is 40 to 50 mesh; and / or the particle size of the green body particles is 10 mm to 50 mm.
[0015] In one example of the present invention, the green body particles are subjected to a melt sintering process, comprising:
[0016] Pre-sintering treatment: pre-sintering the green body particles at a temperature of 700° C. to 800° C. for 1 hour to 2 hours;
[0017] Melting treatment, adding flux to the pre-sintered product, and keeping the temperature at 900° C. to 1050° C. for 0.5 h to 1 h;
[0018] Calcination treatment: adding a chlorine-promoting volatilizer to the product after the melt treatment, calcining at a temperature of 1100° C. to 1300° C. for 1 to 2 hours to obtain a sintered product.
[0019] In one example of the present invention, the flux includes one or more of sodium oxide, potassium oxide, sodium fluoride, potassium fluoride, and calcium oxide; and / or the added amount of the flux accounts for 3% to 6% of the total mass of the medical waste slag, the medical waste fly ash, the red mud and the desulfurization gypsum.
[0020] In one example of the present invention, the chlorine-promoting volatilizer includes one or more of aluminum oxide, iron oxide, and sodium silicate; and / or the added amount of the chlorine-promoting volatilizer accounts for 0.5% to 1% of the total mass of the medical waste slag, the medical waste fly ash, the red mud and the desulfurization gypsum.
[0021] In one example of the present invention, the green body particles are cooled down by air cooling after the melt sintering process, and the temperature is reduced to room temperature within 10 minutes.
[0022] In one example of the present invention, the slag-based cement and silicate cement are mixed and cured, comprising:
[0023] The slag-based cement, the silicate cement and water are mixed and stirred uniformly in a mass ratio of (1-1.5):1:1 to prepare a mixed aqueous solution;
[0024] The mixed aqueous solution is stirred at a speed of 300 to 350 rpm / min for 120 to 180 seconds, standard sand is added and stirred for 120 to 180 seconds, and after being stirred evenly, stirring is continued for not less than 90 seconds to obtain a sample;
[0025] The sample is poured into a mold, cured at room temperature for 24 hours, and then demoulded. The demoulded sample is cured in a standard curing room with constant temperature and humidity for more than 30 days to obtain a gelling material.
[0026] In one example of the present invention, the mass ratio of the standard sand to the slag-based cement is (5-6):1.
[0027] In an example of the present invention, the curing parameters of the constant temperature and humidity standard curing room are: temperature of 20° C. to 30° C., relative humidity RH ≥ 95%.
[0028] The present invention uses slag and fly ash after incineration of medical waste as raw materials, adds red mud and desulfurized gypsum as auxiliary materials, obtains slag-based cement through granulation and high-temperature melting treatment, and then mixes and cures the slag-based cement with ordinary silicate cement to obtain a cementitious material. Medical waste slag and medical waste fly ash can effectively remove heavy metals and chloride salts in the incineration residues through high-temperature melting and co-treatment. At the same time, the prepared cementitious material can replace traditional cement-based materials, which can not only effectively control production costs, but also realize the resource utilization of solid waste, save energy and reduce carbon emissions while reducing the pollution of solid waste to the environment.
[0029] The preparation method of the present invention reduces the heavy metal content of the molten vitrified product of medical waste slag and medical waste fly ash, reduces the risk of heavy metal leaching from the vitrified product, and lays a foundation for subsequent conversion of the vitrified product into an available cementitious material. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 A flow chart of a method for preparing a gelling material according to an embodiment of the present invention;
[0032] Figure 2 A flow chart of a melt sintering process in one embodiment of a method for preparing a cementitious material of the present invention;
[0033] Figure 3 The present invention is a flow chart of the preparation method of the cementitious material of the present invention and the mixing and curing of slag-based cement and silicate cement in one embodiment. DETAILED DESCRIPTION
[0034] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.
[0035] It should be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present invention, and thus the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0036] In the following description, numerous details are discussed to provide a more thorough explanation of the embodiments of the present invention. However, it is obvious to those skilled in the art that the embodiments of the present invention can be implemented without these specific details. In other embodiments, well-known structures and devices are shown in the form of block diagrams rather than in detail to avoid making the embodiments of the present invention difficult to understand.
[0037] The present invention provides a method for preparing a cementitious material, wherein the preparation method uses medical waste incineration slag, medical waste incineration fly ash, red mud and desulfurized gypsum as raw materials, prepares slag-based cement by high-temperature melting, and then mixes and cures the slag-based cement with silicate cement to prepare the final cementitious material. The method has a simple process and low cost, realizes the harmless disposal of medical waste incineration slag and fly ash, and provides a method for converting high-temperature molten products into cementitious materials, thereby realizing the resource utilization of waste.
[0038] See also Figure 1 The method for preparing the gelling material of the present invention comprises at least the following steps:
[0039] S1. Mix and stir medical waste slag, medical waste fly ash, red mud, desulfurized gypsum and slag cooling water to obtain a mixed slurry;
[0040] S2, granulating the mixed slurry and drying it to obtain green body particles;
[0041] S3, melting and sintering the green body particles, cooling them, and then grinding them to obtain slag-based cement;
[0042] S4. Mix and cure the slag-based cement and silicate cement to obtain a cementitious material.
[0043] In step S1, medical waste slag and medical waste fly ash are by-products of medical waste incineration. Among them, medical waste slag is the combustion residue discharged after the incineration of medical waste; medical waste fly ash is the fine particles collected from the flue gas during the incineration process. Medical waste slag and medical waste fly ash contain a large amount of Si, Al, Ga, Fe and other components, which can be used as raw materials for cement production. Red mud is an industrial solid waste discharged after alumina is extracted from bauxite, and its main components include SiO2, Al2O3, CaO, Fe2O3, etc.; desulfurization gypsum is a by-product produced in the flue gas desulfurization process, and its main component is calcium sulfate dihydrate (CaSO4·2H2O). The addition of red mud and desulfurization gypsum can further supplement Si, Al, Ga, F and other components to improve the strength of the material.
[0044] Since large particles of raw materials are not conducive to mixing between the components, the raw materials need to be crushed to obtain small particles before batching. The particle size of each raw material in this step is 40-50 mesh. That is, before batching, the raw materials are first crushed into particles of 40-50 mesh size. There is no restriction on the crushing method here, for example, crushing by a crusher; then filter with a mesh sieve of 40 mesh, 45 mesh or 50 mesh to obtain raw materials that meet the requirements.
[0045] In step S1, the mass ratio of TCM waste slag, medical waste fly ash, red mud and desulfurized gypsum is (1-3): (1-5): (1-2): (1-3), that is, the screened raw materials are mixed evenly according to the above ratio, for example, it can be 1:1:1:1, or 2:3:1.5:2, or 3:5:2:3, etc. Then, slag cooling water is added and mixed evenly, wherein the addition amount of slag cooling water accounts for 1% to 10% of the total mass of the mixed slurry, for example, the addition amount of slag cooling water accounts for 1%, 5%, 8% or 10% of the total mass of the mixed slurry, etc.
[0046] Step S2 is to send the mixed slurry obtained in step S1 into a granulator for granulation to obtain particles with a certain shape, and then dry them to obtain green body particles. Among them, the particle size of the green body particles is 10mm to 50mm, further, the particle size of the green body particles is 20 to 40mm, and further, the particle size of the green body particles is 30mm. The smaller the particle size of the green body particles, the more conducive it is to the subsequent melting process and the compressive strength of the product is improved. The drying method in this step can adopt conventional technical means in the field, for example, baking in an oven at 105°C to constant weight.
[0047] See also Figure 1 and Figure 2 Step S3 is to perform a melting and sintering process on the green body particles. In this embodiment, a multi-stage heating method is adopted. The specific process is as follows:
[0048] S31, pre-sintering treatment, pre-sintering the green body particles at a temperature of 700° C. to 800° C. for 1 h to 2 h.
[0049] In this step, the green body particles are pre-sintered at a low temperature so that the materials adhere to each other and present a preliminary sintered state. The pre-sintering temperature can be controlled at 700°C, 750°C or 800°C, etc. The pre-sintering time can be 1h, 1.5h or 2h, etc.
[0050] S32, melting treatment, adding flux to the pre-sintered material, keeping the temperature at 900°C to 1050°C for 0.5h to 1h.
[0051] This step is to add flux to the pre-sintered material after the pre-sintering treatment to reduce the melting point of the material to 900°C to 1050°C, for example, 900°C, 1000°C or 1050°C, and keep it at its melting point temperature for 0.5h to 1h, for example, 0.5h, 0.8h or 1h, etc. The melting point temperature of the material is related to the content of the added flux.
[0052] In some embodiments, the amount of flux added is 3% to 6% of the mass of the material (the total mass of medical waste slag, medical waste fly ash, red mud and desulfurized gypsum). For example, the amount of flux added is 3%, 5% or 6% of the mass of the material. The flux includes one or more combinations of sodium oxides, potassium oxides, sodium fluorides, potassium fluorides, and calcium oxides. Further, the flux includes one or more of sodium oxide, potassium oxide, calcium oxide, sodium fluoride, potassium fluoride, and calcium oxide. That is, the flux can be selected from any one of the materials listed above, such as sodium oxide or potassium oxide, or it can be a combination of any two or more of the materials listed above, such as a combination of sodium fluoride and calcium oxide, and so on. It should be noted that when the flux includes two or more compositions, there is no restriction on the ratio between the components in the composition, and they can be mixed in any proportion.
[0053] S33, calcination treatment, adding a chlorine-promoting volatilizer to the melt-treated material, calcining at a temperature of 1100° C. to 1300° C. for 1 to 2 hours to obtain a sintered product.
[0054] The addition of the chlorine-promoting volatilizer in this step helps volatilize the chloride salt in the raw material. In some embodiments, the chlorine-promoting volatilizer includes one or more of aluminum oxide, iron oxide, and sodium silicate; that is, the chlorine-promoting volatilizer can be selected from any one of the materials listed above, such as aluminum oxide or iron oxide, etc., or can be selected from any two or three of the materials listed above, such as a combination of aluminum oxide and iron oxide; or a combination of aluminum oxide and sodium silicate. When the chlorine-promoting volatilizer is a combination of two or three, there is no restriction on the ratio between the components in the combination, and they can be mixed in any proportion.
[0055] The amount of the chlorine-promoting volatilizer added affects the volatilization of chloride salts in the molten product. In one embodiment, the amount of the chlorine-promoting additive added accounts for 0.5% to 1% of the material mass (total mass of medical waste slag, medical waste fly ash, red mud and desulfurized gypsum), for example, the amount of the chlorine-promoting additive added accounts for 0.5%, 0.8% or 1% of the material mass, etc.
[0056] The calcination temperature in this step can be, for example, 1100°C, 1200°C or 1300°C, and the calcination time can be 1h, 1.5h or 2h, etc. After the calcination is completed, the temperature is cooled to room temperature to obtain a sintered product. In one embodiment, the cooling method is air cooling, specifically, air cooling by a cold air blower, and the temperature is reduced from the calcination temperature to room temperature within 10 minutes.
[0057] After the cooling is completed, the sintered product is dried and then ground to obtain slag-based cement. Since the sintered product may be sticky and present large particles, it is necessary to add a grinding process to break the sticky large particles into small particles with a particle size of less than 200 mesh, that is, after breaking, filter with a 200-mesh sieve to obtain slag-based cement with a particle size of less than 200 mesh.
[0058] See also Figure 1 and Figure 3 Step S4 is the cement curing step. Specifically, it includes:
[0059] S41. Stir and mix slag-based cement, silicate cement and water in a mass ratio of (1-1.5):1:1 to obtain a mixed aqueous solution.
[0060] In this step, the ratio of slag-based cement, silicate cement and water can be selected from any one of the above ratios, such as 1:1:1; or 1.2:1:1 or 1.5:1:1, etc. The slag-based cement, silicate cement and water are mixed in proportion and stirred evenly.
[0061] S42. Stir the mixed aqueous solution at a speed of 300-350 rpm / min for 120-180 seconds, then add standard sand and continue stirring for 120-180 seconds. After stirring evenly, continue stirring for not less than 90 seconds to obtain a sample.
[0062] The stirring speed in this step can be 300rpm / min, 320rpm / min or 350rpm / min, etc.; the stirring time can be 120s, 150s or 180s, etc. The purpose of adding standard sand is to test the strength of cement. Standard sand is quartz sand that meets the standards after processing. It is used to test the strength of cement mortar and is a universal material necessary for testing the strength of cement. After adding standard sand, stir evenly and continue stirring for no less than 90s to obtain a sample.
[0063] In some embodiments, the mass ratio of standard sand to slag-based cement is (5-6):1. For example, the mass ratio of standard sand to slag-based cement can be 5:1, or 5.5:1, or 6:1, and so on.
[0064] S43, pouring the sample into a mold, curing it at room temperature for 24 hours and then demoulding it, and placing the demoulding sample in a standard constant temperature and humidity curing room for more than 30 days to obtain a cementitious material.
[0065] In one embodiment, the curing parameters of the constant temperature and humidity standard curing room are: temperature of 20°C to 30°C, such as 20°C, 25°C or 30°C, relative humidity RH ≥ 95%, such as RH = 95% or RH = 96%, or RH = 98%, etc.
[0066] After step S4 is completed, the final gelling material can be obtained.
[0067] The present invention uses slag and fly ash after incineration of medical waste as raw materials, and adds red mud, desulfurized gypsum and slag cooling water as auxiliary materials, and then obtains slag-based cement after granulation and melting sintering in sequence, and then mixes the slag-based cement with silicate cement and cures to obtain a cementitious material. The present invention has a simple process, low cost and high resource utilization rate. While realizing the harmless disposal of slag and fly ash from incineration of medical waste, a cementitious material is obtained, and the resource utilization of waste is realized.
[0068] The technical scheme of the present invention is described in detail below through several specific examples and comparative examples. Unless otherwise specified, the raw materials and reagents used in the following examples are all commercially available products, or can be prepared by conventional methods in the art, and the instruments used in the examples are all commercially available.
[0069] Example 1
[0070] This embodiment provides a method for preparing a gelling material, comprising the following steps:
[0071] 1) Mix the medical waste slag, medical waste fly ash, red mud and desulfurized gypsum filtered through a 40-mesh sieve in a mass ratio of 1:3:1:1, add slag cooling water, mix and stir evenly to obtain a mixed slurry; wherein the amount of slag cooling water added accounts for 3% of the total mass of the mixed slurry.
[0072] 2) The uniformly mixed material in step 1) is fed into a granulator for granulation and then dried at 105° C. to obtain green granules with a particle size of 10 mm.
[0073] 3) The green body particles obtained in step 2) are pre-sintered at 700°C for 1 hour, and after the pre-sintering, fluxing materials are added and kept at 900°C for 1 hour, and finally a chlorine-promoting volatilizer is added and calcined at 1300°C for 1 hour; wherein the fluxing agent is potassium oxide, and the amount of potassium oxide added accounts for 3% of the total mass of medical waste slag, medical waste fly ash, red mud and desulfurized gypsum; the chlorine-promoting volatilizer is aluminum oxide, and the amount of aluminum oxide added accounts for 1% of the total mass of medical waste slag, medical waste fly ash, red mud and desulfurized gypsum. The product after high-temperature calcination is cooled by fan cooling, and the temperature is reduced to room temperature within 10 minutes.
[0074] 4) drying the cooled product of step 3), grinding it, and passing it through a 200-mesh sieve to obtain slag-based cement.
[0075] 5) uniformly stirring and mixing slag-based cement: ordinary Portland cement: water in a mass ratio of 1:1:1 to prepare a mixed aqueous solution;
[0076] 6) After the mixed aqueous solution was stirred at 300 rpm / min for 120 seconds, standard sand was added in a ratio of 5:1 between the mass ratio of standard sand and slag-based cement and stirred for 120 seconds. After stirring evenly, stirring was continued for 100 seconds to prepare a sample;
[0077] 7) Pour the sample into the mold, and demould it after curing at room temperature for 24 hours. Place the demoulded sample in a constant temperature and humidity standard curing room for 30 days to obtain the cementitious material. The curing parameters of the constant temperature and humidity standard curing room are: temperature 25°C, relative humidity RH = 95%.
[0078] Example 2
[0079] This embodiment provides a method for preparing a gelling material, comprising the following steps:
[0080] 1) Mix the medical waste slag, medical waste fly ash, red mud and desulfurized gypsum filtered through a 40-mesh sieve in a mass ratio of 3:5:1:2, add slag cooling water, mix and stir evenly to obtain a mixed slurry; wherein the amount of slag cooling water added accounts for 5% of the total mass of the mixed slurry.
[0081] 2) The uniformly mixed material in step 1) is fed into a granulator for granulation and then dried at 105° C. to obtain green granules with a particle size of 30 mm.
[0082] 3) The green body particles obtained in step 2) are pre-sintered at 700°C for 2h, and after the pre-sintering, fluxing materials are added and kept at 1000°C for 1h, and finally a chlorine-promoting volatilizer is added and calcined at 1200°C for 2h; wherein the fluxing agent is a combination of sodium fluoride and calcium oxide, and the mass ratio of sodium fluoride to calcium oxide is 1:1, and the amount of the fluxing agent added accounts for 3% of the total mass of medical waste slag, medical waste fly ash, red mud and desulfurized gypsum; the chlorine-promoting volatilizer is alumina, and the amount of alumina added accounts for 1% of the total mass of medical waste slag, medical waste fly ash, red mud and desulfurized gypsum. The product after high-temperature calcination is cooled by fan cooling, and the temperature is reduced to room temperature within 10 minutes.
[0083] 4) drying the cooled product of step 3), grinding it, and passing it through a 100-mesh sieve to obtain slag-based cement.
[0084] 5) uniformly stirring and mixing slag-based cement: ordinary Portland cement: water in a mass ratio of 1:1:1 to prepare a mixed aqueous solution;
[0085] 6) After the mixed aqueous solution was stirred at 350 rpm / min for 120 seconds, standard sand was added in a ratio of 6:1 between standard sand and slag-based cement and stirred for 160 seconds. After stirring evenly, stirring was continued for 100 seconds to prepare a sample;
[0086] 7) Pour the sample into the mold, and demould it after curing at room temperature for 24 hours. Place the demoulded sample in a constant temperature and humidity standard curing room for 30 days to obtain the cementitious material. The curing parameters of the constant temperature and humidity standard curing room are: temperature 30°C, relative humidity RH = 96%.
[0087] Example 3
[0088] This embodiment provides a method for preparing a gelling material, comprising the following steps:
[0089] 1) Medical waste slag filtered through a 50-mesh sieve, medical waste fly ash, red mud, and desulfurized gypsum are mixed uniformly in a mass ratio of 3:1:2:1, and then slag cooling water is added, mixed and stirred uniformly to obtain a mixed slurry; wherein the amount of slag cooling water added accounts for 8% of the total mass of the mixed slurry.
[0090] 2) The mixed slurry obtained in step 1) is fed into a granulator for granulation and then dried at 105° C. to obtain green granules with a particle size of 20 mm.
[0091] 3) The green body particles obtained in step 2) are pre-sintered at 750°C for 1.5h, and after the pre-sintering, fluxing materials are added and kept at 900°C for 0.5h, and finally a chlorine-promoting volatilizer is added and calcined at 1300°C for 1h; wherein the fluxing agent is calcium oxide, and the amount of calcium oxide added accounts for 5% of the total mass of medical waste slag, medical waste fly ash, red mud and desulfurized gypsum; the chlorine-promoting volatilizer is sodium silicate, and the amount of sodium silicate added accounts for 0.8% of the total mass of medical waste slag, medical waste fly ash, red mud and desulfurized gypsum. The product after high-temperature calcination is cooled by fan cooling, and the temperature is reduced to room temperature within 10 minutes.
[0092] 4) drying the cooled product of step 3), grinding it, and passing it through a 100-mesh sieve to obtain slag-based cement.
[0093] 5) uniformly stirring and mixing slag-based cement: ordinary Portland cement: water in a mass ratio of 1.2:1:1 to prepare a mixed aqueous solution;
[0094] 6) After the mixed aqueous solution was stirred at 300 rpm / min for 180 seconds, standard sand was added according to the mass ratio of standard sand to slag-based cement of 5:1 and stirred for 180 seconds. After stirring evenly, stirring was continued for 100 seconds to prepare a sample;
[0095] 7) Pour the sample into the mold, and demould it after curing at room temperature for 24 hours. Place the demoulded sample in a constant temperature and humidity standard curing room for 30 days to obtain the cementitious material. The curing parameters of the constant temperature and humidity standard curing room are: temperature 30°C, relative humidity RH = 96%.
[0096] Example 4
[0097] 1) Medical waste slag filtered through a 45-mesh sieve, medical waste fly ash, red mud, and desulfurized gypsum are mixed evenly in a mass ratio of 2:3:1.5:3, and then slag cooling water is added, mixed and stirred evenly to obtain a mixed slurry; wherein the amount of slag cooling water added accounts for 10% of the total mass of the mixed slurry.
[0098] 2) The uniformly mixed material in step 1) is fed into a granulator for granulation and then dried at 105° C. to obtain green granules with a particle size of 50 mm.
[0099] 3) The green body particles obtained in step 2) are pre-sintered at 800°C for 1 hour, and after the pre-sintering, fluxing materials are added and kept at 1050°C for 40 minutes, and finally a chlorine-promoting volatilizer is added and calcined at 1100°C for 1.5 hours; wherein the fluxing agent is potassium oxide, and the amount of potassium oxide added accounts for 6% of the total mass of medical waste slag, medical waste fly ash, red mud and desulfurized gypsum; the chlorine-promoting volatilizer is aluminum oxide, and the amount of aluminum oxide added accounts for 0.5% of the total mass of medical waste slag, medical waste fly ash, red mud and desulfurized gypsum. The product after high-temperature calcination is cooled by fan cooling, and the temperature is reduced to room temperature within 10 minutes.
[0100] 4) drying the cooled product of step 3), grinding it, and passing it through a 200-mesh sieve to obtain slag-based cement.
[0101] 5) uniformly stirring and mixing slag-based cement: ordinary Portland cement: water in a mass ratio of 1.5:1:1 to prepare a mixed aqueous solution;
[0102] 6) After the mixed aqueous solution was stirred at 330 rpm / min for 150 seconds, standard sand was added according to a mass ratio of standard sand to slag-based cement of 5.5:1 and stirred for 150 seconds. After stirring evenly, stirring was continued for 100 seconds to prepare a sample;
[0103] 7) Pour the sample into the mold, and demould it after curing at room temperature for 24 hours. Place the demoulded sample in a constant temperature and humidity standard curing room for 30 days to obtain the cementitious material. The curing parameters of the constant temperature and humidity standard curing room are: temperature 25°C, relative humidity RH = 95%.
[0104] Comparative Example 1
[0105] The difference between this comparative example and Example 1 is that red mud and desulfurized gypsum are not added, and other preparation methods and conditions are consistent with those of Example 1.
[0106] Comparative Example 2
[0107] The difference between this comparative example and Example 1 is that the particle size of the embryo particles in step 2) is 55 mm, and the other preparation methods and preparation conditions are consistent with those in Example 1.
[0108] Comparative Example 3
[0109] The difference between Comparative Example 3 and Example 1 is that the cooling method in step 3) adopts water cooling, and the other preparation methods and preparation conditions are consistent with Example 1.
[0110] According to GB / T17671-2020 "Test Method for Cement Mortar Strength (ISO Method)", the molded samples were cured and the compressive strength of samples at different ages was tested. The compressive strength of the slag-based cementitious material of the present invention at different ages, the test results are shown in Table 1.
[0111] Table 1: Compressive strength (MPa) of cementitious materials of Examples 1 to 3 and Comparative Examples 1 to 3
[0112]
[0113]
[0114] It can be concluded from Table 1 that the 3d compressive strength and 28d compressive strength of the cementitious materials prepared in Examples 1 to 4 are close to the parameters of 42.5 ordinary Portland cement, and can be used as a substitute for ordinary cement.
[0115] Compared with Example 1, in Comparative Example 1, no auxiliary materials, red mud and desulfurized gypsum, were added. The 3d compressive strength of the prepared cementitious material was reduced by 18.3%, and the 28d compressive strength was reduced by 15.7%, indicating that the addition of auxiliary materials, red mud and desulfurized gypsum, can improve the compressive strength of the cementitious material.
[0116] Compared with Example 1, in Comparative Example 2, the particle size of the green body particles during granulation is larger, and the 3d compressive strength of the prepared cementitious material is reduced by 24.6%, and the 28d compressive strength is reduced by 15%. This is because the larger the particle size of the green body particles, the smaller the contact area between the particles, which will reduce the bonding force between the particles, thereby affecting the overall strength of the sintered body; at the same time, larger particles are more difficult to rearrange and diffuse during the sintering process, which limits the density of the sintered body and thus affects the strength of the material.
[0117] In Comparative Example 3 compared with Example 1, the cooling method after sintering is changed from air cooling to water cooling. The 3d compressive strength of the cementitious material is reduced by 29.3%, and the 28d compressive strength is reduced by 23%. This is because the cooling rate of water cooling is greater than the cooling rate of air cooling, and rapid cooling will result in insufficient time for the gas inside the material to be discharged, leaving more voids inside the material, thereby reducing the density and compressive strength of the material; and rapid cooling will also generate greater thermal stress inside the material, resulting in the generation or expansion of microcracks, thereby reducing the compressive strength.
[0118] The present invention uses slag and fly ash after incineration of medical waste as raw materials, adds red mud and desulfurized gypsum as auxiliary materials, obtains slag-based cement through granulation and high-temperature melting treatment, and then mixes and cures the slag-based cement with ordinary silicate cement to obtain a cementitious material. The preparation process of the present invention is simple and low in cost. While realizing the harmless disposal of slag and fly ash from incineration of medical waste, a cementitious material that can replace silicate cement is obtained, realizing the resource utilization of waste. Therefore, the present invention effectively overcomes some practical problems in the prior art and has high utilization value and use significance.
[0119] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a gelling material, characterized in that: The following steps are involved: Medical waste slag, medical waste fly ash, red mud, desulfurized gypsum and slag cooling water are mixed and stirred uniformly to prepare a mixed slurry; Granulating the mixed slurry and drying it to obtain green body particles; The green body particles are subjected to melting and sintering treatment, cooled, and then ground to obtain slag-based cement; The slag-based cement is mixed with silicate cement and cured to obtain a cementitious material.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the medical waste slag, medical waste fly ash, red mud and desulfurized gypsum is (1-3): (1-5): (1-2): (1-3); the mass of the slag cooling water accounts for 1% to 10% of the total mass of the mixed slurry.
3. The preparation method according to claim 1, characterized in that: The particle size of the medical waste slag, the medical waste fly ash, the red mud and the desulfurized gypsum is 40 to 50 meshes; and / or the particle size of the green body particles is 10 mm to 50 mm.
4. The preparation method according to claim 1, characterized in that: The green body particles are subjected to a melt sintering process, comprising: Pre-sintering treatment: pre-sintering the green body particles at a temperature of 700° C. to 800° C. for 1 hour to 2 hours; Melting treatment, adding flux to the pre-sintered material, and keeping the temperature at 900° C. to 1050° C. for 0.5 h to 1 h; Calcination treatment: adding a chlorine-promoting volatilizer to the material after the melt treatment, calcining at a temperature of 1100° C. to 1300° C. for 1 to 2 hours to obtain a sintered product.
5. The preparation method according to claim 4, characterized in that: The flux includes one or more of sodium oxide, potassium oxide, sodium fluoride, potassium fluoride, and calcium oxide; and / or the added amount of the flux accounts for 3% to 6% of the total mass of the medical waste slag, the medical waste fly ash, the red mud and the desulfurization gypsum.
6. The preparation method according to claim 4, characterized in that: The chlorine-promoting volatilizer includes one or more of aluminum oxide, iron oxide, and sodium silicate; and / or the added amount of the chlorine-promoting volatilizer accounts for 0.5% to 1% of the total mass of the medical waste slag, the medical waste fly ash, the red mud and the desulfurization gypsum.
7. The preparation method according to claim 1, characterized in that: The green body particles are cooled down after the melt sintering process by using a cooling fan to cool down the temperature to room temperature within 10 minutes.
8. The preparation method according to claim 1, characterized in that: The slag-based cement and silicate cement are mixed and cured, comprising: The slag-based cement, the silicate cement and water are stirred and mixed uniformly in a mass ratio of (1-1.5):1:1 to prepare a mixed aqueous solution; The mixed aqueous solution is stirred at a speed of 300 rpm / min to 350 rpm / min for 120 s to 180 s, standard sand is added and stirred for 120 s to 180 s, and after being stirred evenly, stirring is continued for not less than 90 s to obtain a sample; The sample is poured into a mold, cured at room temperature for 24 hours, and then demoulded. The demoulded sample is cured in a standard curing room with constant temperature and humidity for more than 30 days to obtain a gelling material.
9. The preparation method according to claim 8, characterized in that: The mass ratio of the standard sand to the slag-based cement is (5-6):
1.
10. The preparation method according to claim 8, characterized in that: The curing parameters of the constant temperature and humidity standard curing room are: temperature of 20° C. to 30° C., relative humidity RH ≥ 95%.