Grinding aid suitable for cement with high content of limestone and preparation method of grinding aid

By using specific agitators in high-addition limestone cement, the problems of low grinding efficiency and reduced strength in the later stage are solved, and the effect of improving grinding efficiency and cement performance is achieved.

CN118955001APending Publication Date: 2024-11-15SHANDONG LONGFEI ADDITIVES CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411023085.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

High-addition limestone cement leads to a decrease in the later strength, an increase in initial slump and an increase in particle size during the grinding process, and the grinding efficiency is low, affecting the performance of the cement.

Method used

Using a grinding aid, the raw materials include 10-20% triaxanolamine, 2-10% sulfonate, 2-10% phosphate, 5-10% polyol, 5- 10% acrylamide and 8-15% sugars are prepared by specific stirring steps and temperature control to form a synergistic aid to improve grinding efficiency and particle dispersion.

Benefits of technology

The grinding efficiency and later strength of high-added limestone cement is improved, the 45μm sieve allowance is reduced, the water demand and hydration heat of the cement are reduced, the crack phenomenon is reduced, and the and ease of cement is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004967830580000071
    Figure BDA0004967830580000071
Patent Text Reader

Abstract

The invention discloses a grinding aid suitable for high-volume limestone cement, and also discloses a preparation method of the grinding aid suitable for high-volume limestone cement. The grinding aid comprises the following raw materials: 10-20% of trialkanolamine, 2-10% of sulfonate, 2-10% of phosphate, 5-10% of polyol, 5-10% of acrylamide, 8-15% of saccharides and the balance of deionized water. According to the grinding aid prepared by the invention, through the synergistic effect of active groups contained in various raw materials, the dispersing performance of cement particles with high content of limestone is improved, the later strength of cement is also improved, and the phenomenon that the cement cracks is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of high-dosage limestone cement, and in particular to a grinding aid suitable for high-dosage limestone cement and a preparation method thereof. Background Art

[0002] In construction projects, especially in cement production, fly ash and slag are no longer limited to being used as admixtures. Limestone powder is a waste material produced in the production of crushed stone and stone chips. It has a wide source and is inexpensive. As an admixture in cement production, it can reduce pollution and resource waste, showing huge economic and social benefits.

[0003] However, due to the chemical properties of limestone itself, although it can improve the early strength of cement and improve the water retention and other properties of cement to a certain extent, the addition of a large amount of limestone powder to cement will reduce the later strength of cement, and due to its own properties, the initial slump will increase when the amount of addition increases. In addition, the fine particles produced by limestone during the grinding process will be wrapped on the surface of the clinker fine particles due to the action of various active groups on the surface of the particles, increasing the particle size. Summary of the invention

[0004] To solve the above technical problems, the first aspect of the present invention proposes a grinding aid suitable for high-dosage limestone cement. The raw materials of the grinding aid include, by mass percentage, 10-20% trialkanolamine, 2-10% sulfonate, 2-10% phosphate, 5-10% polyol, 5-10% acrylamide, 8-15% sugar, and deionized water to make up the balance.

[0005] Preferably, the mass percentage of the trialkanolamine is 10-15%.

[0006] Preferably, the trialkanolamine is selected from at least one of triethanolamine, triisopropanolamine and diethanol monoisopropanolamine.

[0007] Preferably, the sulfonate is selected from at least one of alkyl sulfonates, alkylbenzene sulfonates and hydrocarbon sulfonates.

[0008] Preferably, the polyol is selected from at least one of polypropylene glycol, polyethylene glycol and dipropylene glycol.

[0009] Preferably, the acrylamide is selected from at least one of methacrylamide, caprolactam, N-vinylcaprolactam, N,N-dimethylacrylamide and N-hydroxymethylacrylamide.

[0010] Preferably, the sugar is cellulose.

[0011] Preferably, the cellulose is selected from at least one of hydroxypropyl methylcellulose, methyl cellulose ether, hydroxyethyl cellulose ether, hydroxyethyl methyl cellulose ether and carboxymethyl cellulose.

[0012] The second aspect of the present invention provides a method for preparing a grinding aid suitable for high-dosage limestone cement, the preparation steps being as follows:

[0013] (1) Add acrylamide and sugar into deionized water and stir to dissolve;

[0014] (2) Add sulfonate, phosphate, trialkanolamine and polyol and stir evenly to obtain the grinding aid.

[0015] Preferably, the stirring temperature in step (2) is 40-50°C.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1. The grinding aid prepared by the present invention improves the grinding efficiency of the high-admixture limestone cement grinding process through the synergistic effect of various raw materials, and through the joint action of the active groups of each component in the grinding aid, the dispersibility of the high-admixture limestone cement particles is guaranteed, and the 45μm sieve residue of cement is reduced. In addition, the grinding aid prepared by the present invention can also improve the strength of cement, especially improve the later strength of cement.

[0018] 2. The grinding aid prepared by the present invention is used in high-dosage limestone cement to improve the workability of cement, reduce bleeding and segregation, reduce the water demand of cement, further reduce the hydration heat of cement, and reduce the phenomenon of cement cracks.

[0019] 3. The grinding aid prepared by the present invention has a simple preparation method and readily available raw materials, and the grinding aid prepared by the present invention can improve cement performance even when added in small amounts. DETAILED DESCRIPTION

[0020] To solve the above technical problems, the first aspect of the present invention proposes a grinding aid suitable for high-dosage limestone cement. The raw materials of the grinding aid include, by mass percentage, 10-20% trialkanolamine, 2-10% sulfonate, 2-10% phosphate, 5-10% polyol, 5-10% acrylamide, 8-15% sugar, and deionized water to make up the balance.

[0021] Preferably, the mass percentage of the trialkanolamine is 10-15%.

[0022] Preferably, the mass percentage of the trialkanolamine is 10%.

[0023] Preferably, the trialkanolamine is selected from at least one of triethanolamine, triisopropanolamine and diethanol monoisopropanolamine.

[0024] Preferably, the trialkanolamine is diethanol monoisopropanolamine.

[0025] Preferably, the sulfonate is selected from at least one of alkyl sulfonates, alkylbenzene sulfonates and hydrocarbon sulfonates.

[0026] Preferably, the sulfonate is an alkyl sulfonate; more preferably, the alkyl sulfonate is sodium dodecyl sulfonate.

[0027] Preferably, the phosphate is sodium metaphosphate.

[0028] Preferably, the polyol is selected from at least one of polypropylene glycol, polyethylene glycol and dipropylene glycol.

[0029] Preferably, the polyol is polypropylene glycol, purchased from Nanjing Changjiang Jiangyu Oil Co., Ltd., model JY-099.

[0030] Preferably, the acrylamide is selected from at least one of methacrylamide, caprolactam, N-vinylcaprolactam, N,N-dimethylacrylamide and N-hydroxymethylacrylamide.

[0031] Preferably, the acrylamide is N-hydroxymethyl acrylamide.

[0032] Preferably, the sugar is cellulose.

[0033] Preferably, the cellulose is selected from at least one of hydroxypropyl methylcellulose, methyl cellulose ether, hydroxyethyl cellulose ether, hydroxyethyl methyl cellulose ether and carboxymethyl cellulose.

[0034] Preferably, the cellulose is carboxymethyl cellulose.

[0035] Preferably, the grinding aid raw materials include, by mass percentage: 10% diethanol monoisopropanolamine, 2-10% sodium dodecyl sulfate, 2-10% sodium metaphosphate, 5-10% polyglycerol, 5-10% N-hydroxymethyl acrylamide, 8-15% carboxymethyl cellulose, and deionized water to make up the balance.

[0036] Preferably, the grinding aid raw materials include, by mass percentage: 10% diethanol monoisopropanolamine, 2-5% sodium dodecyl sulfate, 2-8% sodium metaphosphate, 5-8% polyglycerol, 5-10% N-hydroxymethyl acrylamide, 8-15% carboxymethyl cellulose, and deionized water to make up the balance.

[0037] Preferably, the mass ratio of diethanol monoisopropanolamine to N-hydroxymethyl acrylamide is 1:(0.5-0.8).

[0038] Preferably, the mass ratio of diethanol monoisopropanolamine to carboxymethyl cellulose is 1:(1-1.5).

[0039] Diethanol monoisopropanolamine is a tertiary amine with a hydroxyalkyl group. Because the nitrogen atom is connected to three hydroxyalkyl groups, the adsorption steric hindrance between the nitrogen atom on diethanol monoisopropanolamine and the cement particles becomes larger, and the hydroxyalkyl group is more likely to adsorb with the active groups on the surface of the cement particles, which affects the fluidity of the cement particles and the strength of the cement. The applicant found in the test process that when N-hydroxymethyl acrylamide and carboxymethyl cellulose and other substances are added to prepare the grinding aid, the fluidity of high-dosage limestone cement and the later strength of the cement can be effectively improved. In particular, when the mass ratio of diethanol monoisopropanolamine to N-hydroxymethyl acrylamide is 1: (0.5-0.8); the mass ratio of diethanol monoisopropanolamine to carboxymethyl cellulose is 1: (1-1.5), the cement fluidity and strength improvement effect is most obvious. The applicant speculates that the possible reason is that carboxymethyl cellulose, N-hydroxymethyl acrylamide, etc. in the grinding aid combine with calcium ions during cement grinding, reducing the adsorption between calcium oxide ions, improving grinding efficiency, and reducing the average particle size; however, when too much carboxymethyl cellulose, N-hydroxymethyl acrylamide, etc. are added, the average particle size is too small, the hydration of cement is accelerated, and the strength of cement is reduced, especially the later strength of cement. At the same time, the applicant speculates that substances such as carboxymethyl cellulose and N-hydroxymethyl acrylamide added to the grinding aid will fill the pores formed by hydrated calcium aluminum sulfate, reduce the porosity of cement, and further improve the strength of cement.

[0040] The second aspect of the present invention provides a method for preparing a grinding aid suitable for high-dosage limestone cement, the preparation steps being as follows:

[0041] (1) Add acrylamide and sugar into deionized water and stir to dissolve;

[0042] (2) Add sulfonate, phosphate, trialkanolamine and polyol and stir evenly to obtain the grinding aid.

[0043] Preferably, the stirring temperature in step (2) is 40-50°C.

[0044] The present invention is described in detail below by way of examples. It is necessary to point out here that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by professionals and technicians in this field based on the content of the present invention above still belong to the scope of protection of the present invention.

[0045] Example 1

[0046] A grinding aid suitable for high-dosage limestone cement is proposed. The raw materials include, by mass percentage, 10% diethanol monoisopropanolamine, 6% sodium dodecyl sulfate, 2% sodium metaphosphate, 5% polyglycerol, 5% N-hydroxymethyl acrylamide, 12% carboxymethyl cellulose, and deionized water to make up the balance.

[0047] A method for preparing a grinding aid suitable for high-dosage limestone cement is also proposed, the steps are as follows:

[0048] (1) adding N-hydroxymethyl acrylamide and carboxymethyl cellulose into deionized water and stirring to dissolve at 55° C.; (2) adding sodium dodecyl sulfate, sodium metaphosphate, diethanol monoisopropanolamine and polyglycerol and stirring to uniformly obtain the grinding aid at 45° C.

[0049] The polypropylene glycol was purchased from Nanjing Changjiang Jiangyu Oil Co., Ltd., model JY-099.

[0050] Carboxymethyl cellulose was purchased from Wuhan Mengqi Technology Co., Ltd., CAS No.: 9000-11-7.

[0051] Example 2

[0052] A grinding aid suitable for high-dosage limestone cement is proposed. The raw materials include, by mass percentage, 10% diethanol monoisopropanolamine, 5% sodium dodecyl sulfate, 2% sodium metaphosphate, 6% polyglycerol, 8% N-hydroxymethyl acrylamide, 15% carboxymethyl cellulose, and deionized water to make up the balance.

[0053] A method for preparing a grinding aid suitable for high-dosage limestone cement is also proposed, the steps are as follows:

[0054] (1) adding N-hydroxymethyl acrylamide and carboxymethyl cellulose into deionized water and stirring to dissolve at 55° C.; (2) adding sodium dodecyl sulfate, sodium metaphosphate, diethanol monoisopropanolamine and polyglycerol and stirring to uniformly obtain the grinding aid at 45° C.

[0055] The polypropylene glycol was purchased from Nanjing Changjiang Jiangyu Oil Co., Ltd., model JY-099.

[0056] Carboxymethyl cellulose was purchased from Wuhan Mengqi Technology Co., Ltd., CAS No.: 9000-11-7.

[0057] Comparative Example 1

[0058] A grinding aid suitable for high-dosage limestone cement is proposed, and a preparation method of the grinding aid suitable for high-dosage limestone cement is also proposed. The specific implementation method is the same as Example 2, except that the addition amount of diethanol monoisopropanolamine is 5%.

[0059] Comparative Example 2

[0060] A grinding aid suitable for high-dosage limestone cement is proposed, and a preparation method of the grinding aid suitable for high-dosage limestone cement is also proposed. The specific implementation method is the same as Example 2, except that the addition amount of diethanol monoisopropanolamine is 25%.

[0061] Comparative Example 3

[0062] A grinding aid suitable for high-dosage limestone cement is proposed, and a preparation method of the grinding aid suitable for high-dosage limestone cement is also proposed. The specific implementation method is the same as Example 2, except that the added amount of carboxymethyl cellulose is 3%.

[0063] Comparative Example 4

[0064] A grinding aid suitable for high-dosage limestone cement is proposed, and a preparation method of the grinding aid suitable for high-dosage limestone cement is also proposed. The specific implementation method is the same as Example 2, except that the added amount of carboxymethyl cellulose is 30%.

[0065] Comparative Example 5

[0066] A grinding aid suitable for high-dosage limestone cement is proposed, and a preparation method of the grinding aid suitable for high-dosage limestone cement is also proposed. The specific implementation method is the same as Example 2, except that the addition amount of N-hydroxymethyl acrylamide is 2%.

[0067] Comparative Example 6

[0068] A grinding aid suitable for high-dosage limestone cement is proposed, and a preparation method of the grinding aid suitable for high-dosage limestone cement is also proposed. The specific implementation method is the same as Example 2, except that the addition amount of N-hydroxymethyl acrylamide is 20%.

[0069] Comparative Example 7

[0070] A grinding aid suitable for high-dosage limestone cement is proposed, and a preparation method of the grinding aid suitable for high-dosage limestone cement is also proposed. The specific implementation method is the same as Example 2, except that N-hydroxymethyl acrylamide and carboxymethyl cellulose are not added.

[0071] Performance Testing

[0072] The grinding aids prepared in the examples and comparative examples were added to cement and ground for 25 minutes, and then passed through a 45 μm sieve. The proportions of the cement components were as follows: 49.9 wt% clinker, 40 wt% limestone, 5 wt% fly ash, 5 wt% gypsum, and 0.1 wt% grinding aid.

[0073] Refer to GB / T1345-2005 to determine the sieve residue.

[0074] With reference to GB / T17671-1999, the compressive strength at 3 days, 28 days and 90 days was measured.

[0075] Refer to GB / T 12959-2008 to determine the heat of cement hydration.

[0076] The measurement data are recorded in Table 1.

[0077] Table 1

[0078]

[0079] The above is only a preferred embodiment of the present invention and is not intended to limit the invention in other forms. Any technician familiar with the profession may use the technical content disclosed above to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A grinding aid suitable for high-dosage limestone cement, characterized in that: The raw materials of the grinding aid include, by mass percentage, 10-20% of trialkanolamine, 2-10% of sulfonate, 2-10% of phosphate, 5-10% of polyol, 5-10% of acrylamide, 8-15% of sugar, and deionized water to make up the balance.

2. The grinding aid according to claim 1, characterized in that The mass percentage of the trialkanolamine is 10-15%.

3. The grinding aid according to claim 2, characterized in that The trialkanolamine is selected from at least one of triethanolamine, triisopropanolamine and diethanol monoisopropanolamine.

4. The grinding aid according to claim 1, characterized in that The sulfonate is selected from at least one of alkyl sulfonates, alkylbenzene sulfonates and hydrocarbon sulfonates.

5. The grinding aid according to claim 1, characterized in that The polyol is selected from at least one of polypropylene glycol, polyethylene glycol and dipropylene glycol.

6. The grinding aid according to claim 1, characterized in that The acrylamide is selected from at least one of methacrylamide, caprolactam, N-vinylcaprolactam, N,N-dimethylacrylamide and N-hydroxymethylacrylamide.

7. The grinding aid according to claim 1, characterized in that The sugars are cellulose.

8. The grinding aid according to claim 7, characterized in that The cellulose is selected from at least one of hydroxypropyl methylcellulose, methyl cellulose ether, hydroxyethyl cellulose ether, hydroxyethyl methyl cellulose ether and carboxymethyl cellulose.

9. A method for preparing a grinding aid suitable for high-dosage limestone cement according to any one of claims 1-2, characterized in that: The preparation steps are as follows: (1) Add acrylamide and sugar into deionized water and stir to dissolve; (2) Add sulfonate, phosphate, trialkanolamine and polyol and stir evenly to obtain the grinding aid.

10. The method for preparing a grinding aid according to claim 9, characterized in that: The stirring temperature in step (2) is 40-50°C.

Citation Information

Patent Citations

  • High-limestone-doping-amount cement grinding aid, and preparation method and application thereof

    CN105036585A

  • Limestone-cement liquid grinding aid and preparation method thereof

    CN105236796A

  • Cement grinding aid

    CN106316202A

  • Application method of caprolactam in cement grinding aid

    CN111533480A

  • Method of milling the Portland clinker for the production of gypsumless Portland cements

    US5125976A