Insulation-free concrete track slab for ballastless track of high-speed railway

By using homologous homogeneous basalt gravel, machined sand and basalt fiber cement to prepare high-insulated concrete, and using basalt fiber reinforced ribs to replace non-prestressed ribs, the problems of insulation performance and impact fatigue resistance of high-speed railway track plates are solved, and the problem of high-speed railway track plates is achieved. The high performance and long life of the track plate simplifies the production process.

CN118955031AActive Publication Date: 2024-11-15RAILWAY CONSTR RES INST OF CHINA ACAD OF RAILWAY SCI CO LTD +1

Patent Information

Application Number
CN202411046192.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The prior art is difficult to provide new concrete track plates that meet the insulation, static mechanical properties and dynamic impact fatigue resistance of high-speed railway track plates without additional insulation measures, and traditional methods may lead to short service life and high production costs.

Method used

High-insulating, high-impact fatigue concrete is prepared by homologous homogeneous basalt gravel, machined sand, modified stone powder and basalt fiber cement, and basalt fiber reinforcement is used to replace all non-prestressed ribs in the track plate, and the steaming and cooking process is abolished to meet the requirements of The demand for high-speed railway construction.

Benefits of technology

It has achieved the meeting of the insulation performance requirements of the track plate without additional insulation measures, improved the static mechanical properties and dynamic impact fatigue resistance, extended the service life of the track plate, simplified the production process and reduced production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955031A_ABST
    Figure CN118955031A_ABST
Patent Text Reader

Abstract

The invention discloses an insulation-free concrete track slab for a ballastless track of a high-speed railway. The insulation-free concrete track slab comprises insulation impact-fatigue-resistant concrete and an insulation steel reinforcement framework, the insulating impact fatigue resistant concrete is composed of basalt macadam, machine-made sand, superfine basalt powder, basalt fiber cement and an early strength component. The insulating steel bar framework is basalt fiber bars and serves as non-prestressed bars in a common concrete track board. Optimized design is carried out on the basis of an existing concrete track plate production technology and production process, additional insulation measures and a steam curing process in the track plate production process are omitted, the production procedures of the track plate are reduced, no extra requirements for the production process and production equipment exist, and the track plate production efficiency is improved. The method has important significance in reducing stress concentration of the concrete track slab and prolonging the service life of the ballastless track, and has wide application prospects in construction of high-speed and long-life high-speed rails.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and more particularly to a concrete track slab for a ballastless track of a non-insulated high-speed railway. Background Art

[0002] High-speed railway trains rely on rails to transmit signals, and the insulation performance of track slabs is one of their important performance indicators. The railway industry standards TB / T 3398-2015, TB / T 3399-2015, and China Railway Corporation enterprise standard Q / CR 567-2017 have made detailed provisions for the insulation performance of CRTS I, II, and III slab ballastless track concrete track slabs widely used in my country: The inductance deviation of the rail impedance of a single track slab of CRTS I slab ballastless track concrete track slab shall not be greater than -3%, and the AC effective resistance deviation shall not be greater than +10%; the relative deviation of the inductance of a single track slab of CRTS II slab ballastless track concrete track slab shall not be greater than ±3%, and the relative deviation of the AC resistance of the rail shall not be greater than 15%; the allowable deviation of the inductance of a single track slab of CRTS III slab ballastless track concrete track slab is ±3%, and the AC effective resistance deviation shall not be greater than 15%.

[0003] In order to avoid the adverse effects of the steel skeleton in the track slab on the signal transmission of high-speed trains and meet the insulation performance requirements of the track slab, the relevant standards stipulate that non-prestressed tendons should use polyethylene heat-shrinkable insulation tubes or epoxy resin coated steel bars, and the resistance of the steel skeleton should not be less than 2MΩ. However, the aging of the heat-shrinkable insulation tubes in the alkaline environment of the track slab and the damage of the epoxy coating of the epoxy resin coated steel bars during the manufacturing process can easily lead to a decrease in the insulation performance of the track slab after a certain number of years of service. At the same time, traditional additional insulation measures can easily lead to stress concentration inside the track slab, reducing the dynamic impact fatigue resistance of the track slab. The design service life of ballastless track is only 60 years, which is lower than the 100-year design service life of the main structure of the bridge. Traditional additional insulation measures are one of the main reasons for its low design service life. With the development of higher-speed high-speed train technology, higher requirements are placed on the insulation performance, dynamic impact fatigue resistance and durability of ballastless track. In order to achieve the same service life of ballastless track and the main structure of high-speed railway bridges, it is urgent to develop ballastless track concrete track slabs with good insulation performance, static mechanical properties that meet the requirements, excellent impact fatigue resistance and good durability.

[0004] The invention patent (authorization notification number CN 108046693 B, authorization announcement date 2020.06.19) discloses a method for preparing highly insulating concrete, which adds polymer emulsion or latex powder, paraffin, asbestos fiber, rubber powder and other components to ordinary concrete to improve the insulation performance of concrete. However, this technology may bring about the adverse effects of reduced concrete strength and reduced working performance, and the static load crack resistance, durability and impact fatigue resistance of the track slab are difficult to guarantee.

[0005] The invention patent application (application publication number CN 102605683 A, application publication date 2012.07.25) discloses an integrally insulated concrete track slab and its preparation technology, which adopts an impregnation treatment technology to prepare a concrete track slab with excellent insulation performance. However, this technology requires the track slab to be placed in an environment not higher than 90°C for drying treatment, which increases the manufacturing process of the track slab. High-temperature treatment may also cause the phase transformation of cement hydration products in the concrete, which is not conducive to the impact fatigue resistance of the track slab. At the same time, in harsh service environments, the surface impregnation treatment material is prone to aging and failure, which may cause the insulation performance of the track slab to decrease, affecting the driving safety of high-speed trains.

[0006] The invention patent (authorization announcement number CN 107443542 B, authorization announcement date 2019.09.10) discloses a FRP prestressed tendon ballastless track slab and its preparation method, which uses steel-continuous fiber composite tendons and traditional high-strength steel bars to form a force-bearing tendon mesh, and the track slab has good insulation and mechanical properties. However, the FRP prestressed tendons used in the invention are made of a variety of fiber composite materials such as basalt fiber, aramid fiber and carbon fiber, and the overall cost is relatively high. At the same time, the manufacturing process of the track slab described in the invention is relatively complicated, and it is difficult to control the construction quality during the track slab manufacturing process.

[0007] The utility model patent (authorization announcement number CN 202610660 U, authorization announcement date 2012.12.19) discloses a concrete track slab without insulation measures, and proposes to use basalt fiber bars, glass fiber bars, and carbon fiber bars as reinforcement bars to replace the ordinary steel skeleton in the track slab, which can ensure the insulation performance of the track slab without additional insulation measures. However, this technology uses reinforcement bars to completely replace the steel bars in the track slab, which may lead to the problem of insufficient overall rigidity of the track slab and excessively high production and manufacturing costs, making it difficult to promote and use.

[0008] Although different technologies and processes are currently available for producing high-insulation concrete and high-insulation concrete track slabs, there is still a lack of new concrete track slab manufacturing technology with excellent performance, reliable technology, controllable costs, and the ability to meet the insulation performance, static mechanical properties and dynamic impact fatigue resistance requirements of higher-speed high-speed railways and longer-life ballastless tracks.

[0009] Therefore, how to provide a concrete track slab for ballastless track of non-insulated high-speed railway, which can not only meet the insulation performance requirements of relevant standards for track slabs without additional insulation measures, but also has higher static mechanical properties and dynamic impact fatigue resistance, is a problem that technical personnel in this field urgently need to solve. Summary of the invention

[0010] In view of this, the present invention provides an insulation-free high-speed railway ballastless track concrete slab, which adopts homogeneous basalt crushed stone, machine-made sand, modified stone powder and basalt fiber cement to prepare high-insulation and high-impact fatigue resistance concrete, and adopts basalt fiber tendons to replace all non-prestressed tendons in the track slab to make the steel skeleton, which is suitable for the construction of high-speed railways with higher speeds and longer lifespans.

[0011] In order to achieve the above object, the present invention adopts the following technical solution:

[0012] An insulation-free high-speed railway ballastless track concrete track slab comprises insulating impact fatigue resistant concrete and an insulating steel bar skeleton;

[0013] The insulating impact fatigue resistant concrete is composed of basalt crushed stone, machine-made sand, ultra-fine basalt stone powder, basalt fiber cement and early strength components;

[0014] The insulating steel bar skeleton is a basalt fiber bar used as a non-prestressed bar in an ordinary concrete track slab.

[0015] The beneficial effect of the above technical solution is that basalt crushed stone and machine-made sand are used as the concrete skeleton of the concrete track slab, ultrafine basalt stone powder is used as the mineral admixture, the proportion of crushed stone, machine-made sand and ultrafine basalt stone powder conforms to the MAA close stacking principle, and the prepared concrete has good insulation and durability.

[0016] Preferably, the insulating impact fatigue resistant concrete uses homogeneous basalt crushed stone, machine-made sand and ultra-fine basalt powder, the maximum particle size of the basalt crushed stone is 31.5 mm, the fineness modulus of the machine-made sand is 2.6-3.1, and the activity index of the ultra-fine basalt powder is greater than 85%. The raw materials used to prepare the concrete of the track plate are the same basalt parent rock, which ensures the overall stability of the track plate.

[0017] Preferably, the basalt parent rock used to make the basalt crushed stone, machine-made sand and ultrafine basalt stone powder has a saturated compressive strength greater than 90 MPa and a volume resistivity greater than 1012 Ω·m.

[0018] Preferably, the volume fraction of the chopped basalt fiber in the basalt fiber cement is 0.25% to 1.5%, the fiber diameter is 10 μm to 25 μm, the tensile strength is 3000 MPa to 5000 MPa, the length is 6 mm to 12 mm, and the 28d flexural strength is greater than 12.0 MPa. The basalt fiber cement formed by homogenizing the chopped basalt fiber and cement is used as an impact fatigue performance improvement component to improve the static mechanical properties and dynamic impact fatigue properties of concrete.

[0019] Preferably, the early strength component is an early strength polycarboxylate water reducer and nano calcium silicate hydrate, the early strength polycarboxylate water reducer is added in an amount of 3.0kg to 8.0kg per cubic meter, and the nano calcium silicate hydrate is added in an amount of 15.0kg to 40.0kg per cubic meter. The steam curing process in the traditional track plate production can be eliminated, and the track plate can be prepared without steam curing.

[0020] Preferably, the basalt fiber reinforcement is a reinforcement skeleton composed of pure basalt fiber reinforcement and steel-basalt fiber composite reinforcement, and the resistance of the reinforcement skeleton is not less than 2MΩ. Pure basalt fiber reinforcement and steel-basalt fiber composite reinforcement are used to replace all non-prestressed reinforcements in the track slab, and together with the prestressed reinforcement, the reinforcement skeleton resistance meets the standard requirements under the condition of canceling additional insulation measures, and the concrete track slab has excellent insulation performance and good static mechanical properties.

[0021] Preferably, the elastic modulus of the pure basalt fiber reinforcement is 40 GPa to 60 GPa, and the ultimate tensile strain is 1.5% to 2.5%.

[0022] Preferably, the inner core of the steel-basalt fiber composite bar is ordinary steel bar, the outer periphery of the ordinary steel bar is coated with basalt fiber, the elastic modulus of the steel-basalt fiber composite bar is 100GPa to 120GPa, and the ultimate tensile strain is 0.8% to 1.1%.

[0023] Preferably, the cracking load levels of the static load tests of the cross section and the longitudinal section of the concrete track slab are both greater than level 1.5, the inductance allowable deviation of the concrete track slab to the rail is ±2%, and the AC effective resistance deviation is no more than 10%.

[0024] It can be seen from the above technical solution that, compared with the prior art, the present invention discloses a non-insulated high-speed railway ballastless track concrete track slab, which has the following beneficial effects:

[0025] 1) The present invention is an optimized design based on the existing concrete track slab production technology and production process, eliminating the need for additional insulation measures and steaming process in the track slab production process, reducing the track slab production process, and having no additional requirements for the production process and production equipment, thereby improving the track slab production efficiency;

[0026] 2) The present invention is of great significance in reducing stress concentration of concrete track slabs and extending the service life of ballastless tracks, and has broad application prospects in the construction of high-speed railways with higher speeds and longer lifespans. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0028] Figure 1 A schematic diagram of the track slab concrete composition provided by the present invention;

[0029] Figure 2 A schematic diagram of the composition of the insulating impact-resistant fatigue concrete provided by the present invention;

[0030] Figure 3 This is a schematic diagram of the composition of the insulating steel bar skeleton provided by the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Embodiment 1:

[0033] The embodiment of the present invention discloses a non-insulated high-speed railway ballastless track concrete track slab, which adopts homogeneous basalt crushed stone, machine-made sand, modified stone powder and basalt fiber cement to prepare high-insulation and high-impact fatigue resistance concrete, and adopts basalt fiber bars to replace all non-prestressed bars in the track slab to make a steel bar skeleton, which is suitable for the construction of high-speed railways with higher speed and longer life, and includes insulating impact fatigue resistance concrete and insulating steel bar skeleton;

[0034] The insulating impact fatigue resistant concrete is composed of basalt crushed stone, machine-made sand, ultra-fine basalt stone powder, basalt fiber cement and early strength components;

[0035] Among them, the insulating impact fatigue resistant concrete uses homogeneous basalt crushed stone, machine-made sand and ultra-fine basalt stone powder. The proportion of basalt crushed stone, machine-made sand and ultra-fine basalt stone powder conforms to the close packing principle of the MAA model.

[0036] The maximum particle size of basalt crushed stone is 31.5mm, the fineness modulus of artificial sand is 2.6-3.1, and the activity index of ultrafine basalt powder is greater than 85%.

[0037] The volume fraction of chopped basalt fiber in basalt fiber cement is 0.25% to 1.5%, the fiber diameter is 10 μm to 25 μm, the tensile strength is 3000 MPa to 5000 MPa, the length is 6 mm to 12 mm, and the 28d flexural strength is greater than 12.0 MPa.

[0038] The early strength components are early strength polycarboxylate water reducer and nano calcium silicate hydrate. The dosage of early strength polycarboxylate water reducer is 3.0kg to 8.0kg per cubic meter, and the dosage of nano calcium silicate hydrate is 15.0kg to 40.0kg per cubic meter.

[0039] In order to further optimize the above technical solution, the basalt parent rock used to make the basalt crushed stone, machine-made sand and ultrafine basalt stone powder has a saturated compressive strength greater than 90 MPa and a volume resistivity greater than 1012 Ω·m.

[0040] The insulating steel bar skeleton is a basalt fiber bar used as a non-prestressed bar in an ordinary concrete track slab.

[0041] The basalt fiber reinforcement is a reinforcement skeleton composed of pure basalt fiber reinforcement and steel-basalt fiber composite reinforcement in any proportion, and the resistance of the reinforcement skeleton is not less than 2MΩ.

[0042] The nominal diameter of pure basalt fiber reinforcement is consistent with the diameter of non-prestressed reinforcement in ordinary concrete track slabs, the elastic modulus is 40GPa~60GPa, and the ultimate tensile strain is 1.5%~2.5%.

[0043] In order to further optimize the above technical solution, the inner core of the steel-basalt fiber composite bar is an ordinary steel bar consistent with the non-prestressed steel bar in the ordinary concrete track slab, and the outer periphery of the ordinary steel bar is coated with basalt fiber. The elastic modulus of the steel-basalt fiber composite bar is 100GPa~120GPa, and the ultimate tensile strain is 0.8%~1.1%.

[0044] The track slab manufactured by this embodiment has been tested and found that the static load test cracking load levels of the cross-section and longitudinal section of the concrete track slab are both greater than level 1.5, the allowable deviation of the inductance of the concrete track slab to the rail is ±2%, and the deviation of the AC effective resistance is no more than 10%.

[0045] The concrete track slab provided in this embodiment is made of basalt crushed stone, machine-made sand and ultra-fine basalt stone powder. The saturated compressive strength of the basalt parent rock for making basalt crushed stone, machine-made sand and ultra-fine basalt stone powder is 180.5 MPa, and the volume resistivity is 1.1×1012Ω·m. The continuous graded crushed stone with a maximum particle size of 31.5 mm produced from the basalt parent rock and the machine-made sand with a fineness modulus of 2.7 are used as the aggregate of the track slab concrete. The ultra-fine basalt stone powder with an activity index of 88% is used as a mineral admixture. The addition amount of the ultra-fine basalt stone powder is 20%, and the packing density is 0.82.

[0046] Basalt fiber cement is used as a component to improve impact fatigue resistance. The volume fraction of basalt fiber in cement is 0.5%. The diameter of the chopped basalt fiber is 12 mm, the length is 10 mm, the tensile strength is 3400 MPa, and the 28d flexural strength of basalt fiber cement is 13.5 MPa.

[0047] Early strength polycarboxylate water reducer (PCE-E) and nano calcium silicate hydrate (NCSH) are used as early strength components, with the PCE-E dosage being 5.0 kg and the NCSH dosage being 15.0 kg per cubic meter of concrete.

[0048] Pure basalt fiber tendons are used to completely replace ordinary non-prestressed tendons. The elastic modulus of pure basalt fiber tendons is 108.1GPa and the ultimate tensile strain is 0.85%.

[0049] The insulated steel bar skeleton is overlapped according to the conventional process, the additional insulation measures of heat shrinkable insulation tube (HSIS) and the steam curing process are cancelled, and the concrete track slab is prepared by conventional production process.

[0050] According to the China Railway Corporation enterprise standard Q / CR567-2017, the steel skeleton resistance is measured to be greater than 2MΩ, meeting the standard requirements.

[0051] The flexural fatigue performance of concrete was tested in accordance with the "Railway Concrete Fatigue Performance Test Procedure". The fatigue life of the insulating impact-resistant fatigue concrete specimen was measured to be 1.882 million times, and the fatigue life of the conventional concrete specimen was 1.109 million times, indicating that the track slab concrete has good impact fatigue resistance.

[0052] The resistivity of track slab concrete was measured by Proceq Resipod four-electrode resistivity meter and was 140.8 kΩ·cm, indicating that track slab concrete has excellent insulation properties.

[0053] According to the enterprise standard Q / CR567-2017 of China Railway Corporation, the AC resistance and inductance of the rail with and without the plate were tested. According to TBT 3579-2022, the static load crack resistance test of the concrete track slab was carried out. The results are shown in Table 1, Table 2 and Table 3:

[0054] Table 1 Track plate AC resistance

[0055]

[0056] Table 2 Track plate AC inductance

[0057]

[0058] Table 3 Track slab cracking load

[0059]

[0060] At different frequencies, the maximum deviation of the AC inductance of the rail of the present invention is -2.42%, and the maximum deviation of the AC resistance is 6.91%, which meets the standard requirements for the insulation performance of the track plate.

[0061] The static load crack resistance design values ​​of the track slab cross-section and longitudinal section are 20kN and 30kN respectively, the cracking load cross-section and longitudinal section test values ​​of the conventional steel frame-heat shrink tubing insulation-conventional concrete track slab are 30kN and 45KN, the cracking load cross-section and longitudinal section test values ​​of the track slab of the present invention are 40kN and 55kN respectively, and the cracking load grades are 2.0 and 1.83 respectively, indicating that the track slab has good static mechanical properties.

[0062] After evaluation, it was found that the present invention eliminates the steaming process of conventional track slabs, and the concrete track slabs have excellent insulation properties, good static mechanical properties and high dynamic impact fatigue resistance.

[0063] Embodiment 2:

[0064] The embodiment of the present invention discloses a non-insulated high-speed railway ballastless track concrete track slab, which is different from the embodiment 1 in that:

[0065] Continuously graded crushed stone with a maximum particle size of 20 mm and a fine aggregate with a fineness modulus of 2.8 produced from basalt parent rock with a saturated compressive strength of 200.5 MPa and a volume resistivity of 1.05×1012 Ω·m is used as coarse and fine aggregates for track slab concrete. Ultrafine basalt stone powder with an activity index of 85% is used as mineral admixture. The dosage of ultrafine basalt stone powder is 15%, and the packing density is 0.85.

[0066] Basalt fiber cement is used as a component to improve impact fatigue resistance. The volume fraction of basalt fiber in cement is 0.5%. The diameter of the chopped basalt fiber is 10 mm, the length is 8 mm, the tensile strength is 4100 MPa, and the 28d flexural strength of basalt fiber cement is 14.2 MPa.

[0067] PCE-E and NCSH are used as early strength components, with the PCE-E content being 6.0 kg and the NCSH content being 30.0 kg per cubic meter of concrete.

[0068] Basalt fiber composite bars are used to replace transverse non-prestressed bars, and pure basalt fiber bars are used to replace longitudinal non-prestressed bars. The elastic modulus of the basalt fiber composite bars is 111.7 GPa, and the ultimate tensile strain is 0.93%. The elastic modulus of the pure basalt fiber bars is 44.1 GPa, and the ultimate tensile strain is 2.1%.

[0069] The insulated steel bar skeleton is overlapped according to the conventional process, the additional insulation measures of heat shrinkable insulation tube (HSIS) and the steam curing process are cancelled, and the concrete track slab is prepared by conventional production process.

[0070] According to the China Railway Corporation enterprise standard Q / CR567-2017, the steel skeleton resistance is measured to be greater than 2MΩ, meeting the standard requirements.

[0071] The flexural fatigue performance of concrete was tested in accordance with the "Railway Concrete Fatigue Performance Test Procedure", and the fatigue life of the insulating impact-resistant fatigue concrete specimen was measured to be 1.753 million times, indicating that the track slab concrete has good impact fatigue resistance.

[0072] The resistivity of track slab concrete was measured by Proceq Resipod four-electrode resistivity meter and was 160.4 kΩ·cm, indicating that track slab concrete has excellent insulation properties.

[0073] According to the enterprise standard Q / CR567-2017 of China Railway Corporation, the AC resistance and inductance of the rail with and without the plate were tested. According to TBT 3579-2022, the static load crack resistance test of the concrete track slab was carried out. The results are shown in Table 4, Table 5 and Table 6:

[0074] Table 4 Track plate AC resistance

[0075]

[0076] Table 5 Track plate AC inductance

[0077]

[0078] Table 6 Track slab cracking load

[0079]

[0080] At different frequencies, the maximum deviation of the AC inductance of the rail of the present invention is 2.32%, and the maximum deviation of the AC resistance is 7.36%, which meets the standard requirements for the insulation performance of the track plate.

[0081] The static load crack resistance design values ​​of the track slab cross section and longitudinal section are 20kN and 30kN respectively. The cracking load cross section and longitudinal section test values ​​of the track slab of the present invention are 45kN and 55kN respectively. The cracking load levels are 2.25 and 1.83 respectively, indicating that the track slab has good static mechanical properties.

[0082] After evaluation, it was found that the present invention eliminates the steaming process of conventional track slabs, and the concrete track slabs have excellent insulation properties, good static mechanical properties and high dynamic impact fatigue resistance.

[0083] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0084] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A non-insulated high-speed railway ballastless track concrete track slab, characterized in that: Includes insulated impact fatigue resistant concrete and insulated steel reinforcement skeleton; The insulating impact fatigue resistant concrete is composed of basalt crushed stone, machine-made sand, ultra-fine basalt stone powder, basalt fiber cement and early strength components; The insulating steel bar skeleton is a basalt fiber bar used as a non-prestressed bar in an ordinary concrete track slab.

2. The non-insulated high-speed railway ballastless track concrete track slab according to claim 1, characterized in that: The insulating impact fatigue resistant concrete adopts homogeneous basalt crushed stone, machine-made sand and ultra-fine basalt powder. The maximum particle size of the basalt crushed stone is 31.5 mm, the fineness modulus of the machine-made sand is 2.6-3.1, and the activity index of the ultra-fine basalt powder is greater than 85%.

3. The non-insulated high-speed railway ballastless track concrete track slab according to claim 2, characterized in that: The basalt parent rock used to make the basalt crushed stone, machine-made sand and ultra-fine basalt stone powder has a saturated compressive strength greater than 90 MPa and a volume resistivity greater than 1012 Ω·m.

4. The non-insulated high-speed railway ballastless track concrete track slab according to claim 2, characterized in that: The basalt fiber cement chopped basalt fiber has a volume fraction of 0.25% to 1.5%, a fiber diameter of 10 μm to 25 μm, a tensile strength of 3000 MPa to 5000 MPa, a length of 6 mm to 12 mm, and a 28d flexural strength greater than 12.0 MPa.

5. The non-insulated high-speed railway ballastless track concrete slab according to claim 4, characterized in that: The early strength component comprises an early strength polycarboxylate water reducer and nano calcium silicate hydrate. The early strength polycarboxylate water reducer is added in an amount of 3.0kg to 8.0kg per cubic meter, and the nano calcium silicate hydrate is added in an amount of 15.0kg to 40.0kg per cubic meter.

6. The non-insulated high-speed railway ballastless track concrete track slab according to claim 1, characterized in that: The basalt fiber reinforcement is a reinforcement skeleton composed of pure basalt fiber reinforcement and steel-basalt fiber composite reinforcement, and the resistance of the reinforcement skeleton is not less than 2MΩ.

7. The non-insulated high-speed railway ballastless track concrete slab according to claim 6, characterized in that: The elastic modulus of the pure basalt fiber reinforcement is 40 GPa to 60 GPa, and the ultimate tensile strain is 1.5% to 2.5%.

8. The non-insulated high-speed railway ballastless track concrete slab according to claim 7, characterized in that: The inner core of the steel-basalt fiber composite bar is ordinary steel bar, the outer periphery of the ordinary steel bar is coated with basalt fiber, the elastic modulus of the steel-basalt fiber composite bar is 100GPa-120GPa, and the ultimate tensile strain is 0.8%-1.1%.

9. The non-insulated high-speed railway ballastless track concrete slab according to any one of claims 1 to 8, characterized in that: The cracking load levels of the cross-section and longitudinal section static load tests of the concrete track slab are both greater than level 1.

5. The inductance allowable deviation of the concrete track slab to the rail is ±2%, and the AC effective resistance deviation is no more than 10%.

Citation Information

Patent Citations

  • Impact-resistant basalt fiber reinforced concrete and preparation method thereof

    CN111439977A

  • Bendable concrete and preparation method thereof

    CN113754383A

  • Basalt debris concrete and preparation method thereof

    CN113816666A

  • Steam-curing-free ballastless track concrete composite track plate as well as preparation method and application thereof

    CN115557749A

  • Uninsulated concrete slab track

    CN202610660U

Cited By

  • Anti-fatigue ballastless track concrete under high geothermal environment and preparation method of anti-fatigue ballastless track concrete

    CN121651829A