Water retention type slope curing agent as well as preparation method and application thereof
By using materials such as acrylate copolymer emulsions, cement, fly ash and nano-silica, a dense waterproof layer is formed, which solves the problem of insufficient hardness and water resistance of the water-based emulsion soil curing agent, and achieves high water resistance and impact resistance. Effectively prevent soil erosion and slope landslide.
Patent Information
- Application Number
- CN202411000411.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
AI Technical Summary
The hardness and water resistance of existing aqueous emulsion soil curing agents are insufficient, resulting in difficult to effectively solve the problems of soil erosion and slope landslides.
Materials such as acrylate copolymer emulsion, cement, fly ash and nano-silica are used to form a dense waterproof layer through stirring and spraying, which improves the water resistance and impact resistance of the slope curing agent.
It significantly improves the water resistance and film formation strength of slope curing agent, solves the problems of soil erosion and slope landslide, and is convenient to construct and has no impact on plant growth.
Smart Images

Figure CN118955042A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of slope protection, and particularly relates to a water-retaining slope curing agent and a preparation method and application thereof. Background Art
[0002] At present, slope solidifiers are mainly made of inorganic materials mixed in a certain ratio. Compared with inorganic solidifiers, water-based emulsion solidifiers have a certain gap in hardness and water resistance. This is also one of the main reasons that have been restricting the development of water-based emulsion slope solidifiers. Therefore, how to improve the hardness and water resistance of water-based emulsion soil solidifiers has become an urgent factor.
[0003] Chinese patent CN114907088A introduces a curing agent prepared by using P.O32.5 grade cement, S95 grade slag powder, powdered quicklime, F type fly ash, and desulfurized gypsum; Chinese patent CN114409340A introduces a curing agent mainly composed of silicate cement and added with graphene interpenetrating material, and the graphene sheet structure is highly active and can improve the strength; the above-mentioned types of curing agents are all inorganic curing agents, and although their strength is guaranteed to a certain extent, their dosage is large, and the raw materials need to be mechanically stirred and proportioned, which has certain difficulties in engineering application. Summary of the invention
[0004] In order to solve the problem of insufficient hardness and water resistance of existing water-based emulsion soil solidifiers, the present invention provides a water-retaining slope solidifier, which has strong water resistance and high film-forming strength and can solve the problems of soil erosion and slope landslide to a great extent.
[0005] The invention also provides a preparation method and application of a water-retaining slope curing agent.
[0006] The present invention is achieved through the following technical solutions:
[0007] The present invention provides a water-retaining slope curing agent. The raw materials for preparing the slope curing agent are as follows, measured by mass:
[0008] Acrylate copolymer emulsion 50-60 parts; water 50-60 parts; wetting agent 0.1-0.2 parts; dispersant 0.6-1.0 parts; pH adjuster 0.2-0.3 parts;
[0009] The raw materials for preparing the slope curing agent also include cement, fly ash and nano silicon dioxide, wherein the total mass of the cement and the fly ash is 0.1% to 0.5% of the mass of the acrylic copolymer emulsion, and the mass of the nano silicon dioxide is 0.4% to 1.5% of the mass of the acrylic copolymer emulsion.
[0010] Furthermore, the cement includes at least one of 325 cement, 425 cement and 625 cement, and the nano-silicon dioxide includes at least one of SP15, SP30, SP50, SP30T, SP30S and SP30F.
[0011] Furthermore, the raw materials for preparing the acrylic copolymer emulsion include deionized water, an emulsifier, a reactive surfactant, styrene, methyl methacrylate, a first monomer, methacrylic acid, ammonium persulfate, an initiator, sodium bicarbonate and an inhibitor;
[0012] Among them, the mass ratio of deionized water, emulsifier, reactive surfactant, styrene, methyl methacrylate, first monomer, methacrylic acid, ammonium persulfate, initiator, sodium bicarbonate and inhibitor is (600-700): (4-5): (5-8): (37-40): (70): (185-190): (5-10): 1.5: (1-1.5:) 3: (0.8-2).
[0013] Further, the first monomer includes at least one of butyl acrylate, methyl acrylate, ethyl acrylate, methyl 2-methacrylate, ethyl 2-methacrylate, a-cyanoacrylate, hydroxypropyl acrylate, methacrylic acid, acrylic acid, methyl methacrylate and propyl methacrylate;
[0014] The emulsifier includes at least one of sodium lauryl sulfate, sodium lauryl sulfonate, sodium dodecylbenzene sulfonate and dodecylphenol polyoxyethylene ether;
[0015] The reactive surfactant includes at least one of double-bond alcohol ether sulfosuccinic acid sodium salt, 2-acrylamide-2 methyl isopropyl sodium sulfonate, methyl allyl hydroxypropane sodium sulfonate, sodium vinyl sulfonate and sodium allyloxy hydroxypropane sodium sulfonate.
[0016] Furthermore, the preparation method of the acrylic ester copolymer emulsion is as follows:
[0017] Deionized water, an emulsifier, a reactive surfactant and sodium bicarbonate are placed in a reaction device, stirred and heated;
[0018] Add styrene, methyl methacrylate, the first monomer, methacrylic acid and an initiator into the reaction device, stir and react at a reaction temperature of 70-78° C. for 2.5 hours;
[0019] Adding a polymerization inhibitor into the reaction device to obtain an acrylate copolymer emulsion.
[0020] Further, the initiator includes at least one of ammonium persulfate, potassium persulfate, azobisisobutylamidine hydrochloride and azobisisobutylimidazoline hydrochloride, and the inhibitor includes at least one of hydroquinone, p-tert-butylcatechol, 2,6-di-tert-butyl-p-methylphenol, 4,4'-dihydrobiphenyl and bisphenol A.
[0021] Furthermore, the wetting agent includes at least one of ethanol, propylene glycol, glycerin, disodium lauryl sulfosuccinate, disodium cocoyl monoethanolamide sulfosuccinate and monolauryl phosphate; the dispersant includes at least one of sodium carboxymethyl cellulose, sodium pyrophosphate, sodium hexametaphosphate and polyvinyl alcohol; the pH adjuster includes at least one of ammonia water, sodium carbonate, sodium bicarbonate, calcium carbonate and calcium bicarbonate.
[0022] Based on the same inventive concept, the present invention provides a method for preparing a water-retaining slope curing agent, the preparation method comprising:
[0023] The acrylic copolymer emulsion, deionized water, a wetting agent, a dispersant, a pH regulator, cement, fly ash and nano silicon dioxide are uniformly mixed to obtain the water-retaining slope curing agent.
[0024] Based on the same inventive concept, the present invention also provides an application of a water-retaining slope solidifying agent in preventing soil slope landslides or water soil loss.
[0025] Furthermore, the application includes:
[0026] The water-retaining slope solidifying agent is evenly sprayed on the soil slope to be constructed. The amount of the water-retaining slope solidifying agent is 250-500g / m 2 .
[0027] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0028] The invention discloses a water-retaining slope curing agent, which uses cement and fly ash as aggregates, nano silicon dioxide as an anti-ultraviolet protective agent, and acrylic copolymer emulsion as a binder and a water-retaining component. The invention uses liquid and solid as a mixture, and the skeleton material can provide a certain impact resistance; the polymer emulsion can be quickly cured on the soil surface to form a dense waterproof layer, and provides a certain adhesion, so that the skeleton material has flexibility and improves the impact resistance; the nano silicon dioxide can provide strong anti-ultraviolet performance, so that the curing agent can not be degraded for a long time under high ultraviolet conditions and maintains performance; the slope curing agent of the invention has good soil versatility, a simple formula, convenient construction, and no influence on plant growth. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0030] Figure 1 This is a rainfall simulation test diagram of the present invention. DETAILED DESCRIPTION
[0031] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.
[0032] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.
[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0034] The following will describe in detail a water-retaining slope curing agent, a preparation method and an application thereof in combination with embodiments and experimental data.
[0035] Example 1
[0036] The present embodiment provides a method for preparing a water-retaining slope curing agent, comprising the following steps:
[0037] (1) 700 parts of deionized water, 5 parts of sodium dodecylbenzene sulfonate, 5 parts of sodium alcohol ether sulfosuccinate, and 3 parts of sodium bicarbonate were placed in a reaction apparatus, stirred, and heated;
[0038] (2) Add 40 parts of styrene, 70 parts of methyl methacrylate, 190 parts of butyl acrylate, 10 parts of methacrylic acid, and 1 part of initiator ammonium persulfate into the reaction device, stir and react at a reaction temperature of 75° C. for 2.5 hours;
[0039] (3) adding 0.8 parts of hydroquinone as a polymerization inhibitor to obtain an acrylate copolymer emulsion;
[0040] (4) The acrylic copolymer emulsion is mixed with deionized water, a wetting agent, a dispersant, a pH adjuster, cement, fly ash and nano-silicon dioxide and stirred for 30 minutes to obtain the water-retaining slope curing agent.
[0041] In the raw materials for preparing the water-retaining slope curing agent, the mass fractions of each component are as follows:
[0042] 50 parts of acrylic copolymer emulsion; 50 parts of water; 0.1 parts of propylene glycol as a wetting agent; 0.6 parts of polyvinyl alcohol as a dispersant; 0.2 parts of ammonia water as a pH adjuster; 0.2 parts of 425 cement, 0.1 parts of fly ash, and 0.5 parts of SP30 nano-silicon dioxide.
[0043] Example 2
[0044] In this example, the water-retaining slope curing agent prepared in Example 1 was evenly sprayed on the slope surface at a curing agent dosage of 250 g / ㎡, and a rainfall simulation test was carried out.
[0045] Example 3
[0046] In this example, the water-retaining slope curing agent prepared in Example 1 was evenly sprayed on the slope surface at a curing agent dosage of 500 g / ㎡, and a rainfall simulation test was carried out.
[0047] Comparative Example 1
[0048] In this comparative example 1, the slope curing agent in the above-mentioned embodiment 2 is replaced by an equal amount of polyacrylamide, which is evenly sprayed on the slope surface, and a rainfall simulation test is carried out.
[0049] The rainfall simulation test described in Examples 2, 3 and Comparative Example 1 has the following contents: Figure 1 As shown in the figure, a rapid impact test was conducted on the inclined surface, using a flushing hydraulic with a flow rate of 84 m / s and a flow rate of 0.165×10 -3 m 3 / s, and the impact force is F = 0.06N. This is to simulate the destructive effect of rainfall on the slope.
[0050] The rainfall simulation test results of Examples 2, 3 and Comparative Example 1 are shown in Table 1.
[0051] Table 1
[0052]
[0053] As shown in Table 1, the curing agent prepared in Example 2 can withstand 37.6 minutes of rainfall erosion. With the increase in the amount of slope curing agent used, Example 3 can achieve better results than Example 2. The tolerance time of Comparative Example 1 is 0.5 minutes, which is much lower than that of Examples 2 and 3.
[0054] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.
[0055] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0056] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A water-retaining slope curing agent, characterized in that: The raw materials for preparing the slope curing agent are as follows, in parts by mass: Acrylate copolymer emulsion 50-60 parts; water 50-60 parts; wetting agent 0.1-0.2 parts; dispersant 0.6-1.0 parts; pH adjuster 0.2-0.3 parts; The raw materials for preparing the slope curing agent also include cement, fly ash and nano silicon dioxide, wherein the total mass of the cement and the fly ash is 0.1% to 0.5% of the mass of the acrylic copolymer emulsion, and the mass of the nano silicon dioxide is 0.4% to 1.5% of the mass of the acrylic copolymer emulsion.
2. A water-retaining slope curing agent according to claim 1, characterized in that: The cement includes at least one of 325 cement, 425 cement and 625 cement, and the nano-silicon dioxide includes at least one of SP15, SP30, SP50, SP30T, SP30S and SP30F.
3. A water-retaining slope curing agent according to claim 1, characterized in that: The raw materials for preparing the acrylic copolymer emulsion include deionized water, an emulsifier, a reactive surfactant, styrene, methyl methacrylate, a first monomer, methacrylic acid, ammonium persulfate, an initiator, sodium bicarbonate and an inhibitor; Among them, the mass ratio of deionized water, emulsifier, reactive surfactant, styrene, methyl methacrylate, first monomer, methacrylic acid, ammonium persulfate, initiator, sodium bicarbonate and inhibitor is (600-700): (4-5): (5-8): (37-40): (70): (185-190): (5-10): 1.5: (1-1.5:) 3: (0.8-2).
4. A water-retaining slope curing agent according to claim 3, characterized in that: The first monomer comprises at least one of butyl acrylate, methyl acrylate, ethyl acrylate, methyl 2-methacrylate, ethyl 2-methacrylate, α-cyanoacrylate, hydroxypropyl acrylate, methacrylic acid, acrylic acid, methyl methacrylate and propyl methacrylate; The emulsifier includes at least one of sodium lauryl sulfate, sodium lauryl sulfonate, sodium dodecylbenzene sulfonate and dodecylphenol polyoxyethylene ether; The reactive surfactant includes at least one of double-bond alcohol ether sulfosuccinic acid sodium salt, 2-acrylamide-2 methyl isopropyl sodium sulfonate, methyl allyl hydroxypropane sodium sulfonate, sodium vinyl sulfonate and sodium allyloxy hydroxypropane sodium sulfonate.
5. A water-retaining slope curing agent according to claim 3, characterized in that: The preparation method of the acrylic ester copolymer emulsion is as follows: Deionized water, an emulsifier, a reactive surfactant and sodium bicarbonate are placed in a reaction device, stirred and heated; Add styrene, methyl methacrylate, the first monomer, methacrylic acid and an initiator into the reaction device, stir and react at a reaction temperature of 70-78° C. for 2.5 hours; Adding a polymerization inhibitor into the reaction device to obtain an acrylate copolymer emulsion.
6. A water-retaining slope curing agent according to claim 3, characterized in that: The initiator includes at least one of ammonium persulfate, potassium persulfate, azobisisobutylamidine hydrochloride and azobisisobutylimidazoline hydrochloride, and the inhibitor includes at least one of hydroquinone, p-tert-butylcatechol, 2,6-di-tert-butyl-p-methylphenol, 4,4'-dihydrobiphenyl and bisphenol A.
7. A water-retaining slope curing agent according to claim 1, characterized in that: The wetting agent includes at least one of ethanol, propylene glycol, glycerin, disodium lauryl sulfosuccinate, disodium cocoyl monoethanolamide sulfosuccinate and monolauryl phosphate; the dispersant includes at least one of sodium carboxymethyl cellulose, sodium pyrophosphate, sodium hexametaphosphate and polyvinyl alcohol; the pH adjuster includes at least one of ammonia water, sodium carbonate, sodium bicarbonate, calcium carbonate and calcium bicarbonate.
8. A method for preparing a water-retaining slope curing agent according to any one of claims 1 to 7, characterized in that: The preparation method comprises: The acrylic copolymer emulsion, deionized water, a wetting agent, a dispersant, a pH regulator, cement, fly ash and nano silicon dioxide are uniformly mixed to obtain the water-retaining slope curing agent.
9. Use of a water-retaining slope solidifying agent as claimed in any one of claims 1 to 7 in preventing soil slopes from landslides or preventing soil erosion.
10. The use according to claim 9, characterized in that: The applications include: The water-retaining slope solidifying agent is evenly sprayed on the soil slope to be constructed. The amount of the water-retaining slope solidifying agent is 250-500g / m 2 .
Citation Information
Cited By
Loess slope reinforcement mechanical evaluation method and system and slope reinforcement method
CN121068888A
A mechanical evaluation method and system for loess slope reinforcement
CN121068888B