Low-energy-consumption high-strength high-toughness soft porcelain and preparation method thereof
By using the combined structure and optimized formula of the bottom layer, middle layer and surface layer in soft porcelain, the problems of fragility and insufficient performance in traditional ceramic tiles are solved, and the balance of low energy consumption, high strength and high flexibility is achieved, and the softness is improved The overall performance and service life of porcelain.
Patent Information
- Application Number
- CN202411042129.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional ceramic tiles are fragile and not easy to bend during construction, and it is difficult to take into account both high strength and high flexibility, resulting in high energy consumption and insufficient performance.
Using low-energy consumption, high-strength, high-toughness, and high-toughness soft porcelain composed of the bottom layer, intermediate layer and surface layer, the slurry formula of the bottom layer and surface layer is optimized, including cement, emulsion, quartz sand, silicon carbide, metal microfiber and calcium powder. The intermediate layer is The glass fiber mesh has a curing temperature as low as 110-120℃ and a curing time as short as 50-55min, ensuring high strength and high flexibility.
It achieves a balance of low energy consumption, high strength and high flexibility, reduces production energy consumption, avoids deformation problems caused by high temperature curing, and improves the overall performance and service life of soft porcelain.
Abstract
Description
Technical Field
[0001] The invention relates to the field of building decoration materials, and in particular to a low-energy-consumption, high-strength, high-toughness soft porcelain and a preparation method thereof. Background Art
[0002] In the field of building decoration materials, traditional tiles have long been dominant due to their hardness, wear resistance and easy cleaning. However, with the continuous advancement of building material technology, the limitations of traditional tiles have gradually emerged, such as their fragility and difficulty in bending during construction.
[0003] In order to solve the above problems, soft porcelain has emerged as a new type of building decoration material. It not only retains the beautiful appearance of traditional ceramic tiles, such as imitation stone and imitation wood grain, but also performs well in flexibility, earthquake resistance and crack resistance, solving the problems of traditional ceramic tiles being fragile and difficult to bend during construction, making it increasingly popular and widely used in scenes such as exterior walls, interior walls and floors.
[0004] Although soft porcelain has many advantages, it also has some challenges. For example, in the production process of soft porcelain, in order to ensure its quality and performance, it is usually necessary to cure it at a temperature above 150°C for 60 to 90 minutes, which not only leads to high energy consumption, but also easily causes the soft porcelain to deform at high temperatures, resulting in reduced flexibility. In addition, as a building decoration material, soft porcelain not only needs to have a certain degree of softness to adapt to the deformation and cracks on the building surface, but also needs to have sufficient strength to withstand wind and rain erosion and human damage. However, since flexibility is related to elastic modulus and deformation capacity, that is, the lower the elastic modulus, the stronger the deformation capacity and the higher the flexibility, while too low elastic modulus and deformation capacity will lead to lower strength, making it difficult for soft porcelain to take into account both flexibility and strength. Summary of the invention
[0005] One of the purposes of the present invention is to provide a low-energy consumption, high-strength and high-toughness soft porcelain, which has high toughness and strength, so that the soft porcelain can simultaneously take into account low energy consumption, high strength and high flexibility to overcome the shortcomings of the prior art.
[0006] The second purpose of the present invention is to propose a method for preparing soft porcelain with low energy consumption, high strength and high toughness, wherein the curing temperature is as low as 110-120°C, the curing time is as low as 50-55 minutes, the steps are simple and the operability is strong, which is conducive to reducing the energy consumption of soft porcelain while having high strength and high flexibility.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] A low-energy-consumption, high-strength, high-toughness soft porcelain, comprising a bottom layer, an intermediate layer, and a surface layer arranged in sequence from bottom to top; the bottom layer is obtained by solidifying the bottom layer slurry, the intermediate layer is a glass fiber mesh, and the surface layer is obtained by solidifying the surface layer slurry;
[0009] Calculated by weight, the base slurry includes 3 to 5 parts of cement, 8 to 10 parts of emulsion, 45 to 53 parts of quartz sand, 12 to 20 parts of silicon carbide, 20 to 22 parts of calcium powder, 10 to 15 parts of water and 8 to 10 parts of water reducing agent;
[0010] Calculated by mass, the surface layer slurry includes 3-5 parts of cement, 8-10 parts of emulsion, 55-60 parts of quartz sand, 5-10 parts of silicon carbide, 6-12 parts of metal microfibers, 20-22 parts of calcium powder, 10-15 parts of water and 8-10 parts of water reducing agent.
[0011] Furthermore, the metal microfiber has a diameter of 1 to 30 μm and a length of 0.3 to 0.5 cm.
[0012] Furthermore, the metal microfibers include any one of stainless steel microfibers, silver microfibers and aluminum microfibers.
[0013] Furthermore, the mesh sizes of the quartz sand in the base slurry and the surface slurry are both 60-325 meshes, the mesh sizes of the silicon carbide are both 70-120 meshes, and the mesh sizes of the calcium powder are both 380-400 meshes.
[0014] Furthermore, the emulsions in the base slurry and the surface slurry include at least one of silicone-acrylic emulsion, pure acrylic emulsion and styrene-acrylic emulsion.
[0015] Furthermore, the cement in the base layer slurry and the surface layer slurry is white PO 42.5R cement.
[0016] Furthermore, the thickness of the bottom layer is 0.5-1 mm, the thickness of the middle layer is 0.2-0.5 mm, and the thickness of the surface layer is 2-3 mm.
[0017] Furthermore, the bottom slurry and the surface slurry both include a defoaming agent;
[0018] Calculated by weight, the base slurry includes 3-5 parts of cement, 8-10 parts of emulsion, 45-53 parts of quartz sand, 15-18 parts of silicon carbide, 20-22 parts of calcium powder, 10-15 parts of water, 8-10 parts of water reducer and 2-3 parts of defoamer;
[0019] Calculated by mass, the surface layer slurry includes 3-5 parts of cement, 8-10 parts of emulsion, 55-60 parts of quartz sand, 8-10 parts of silicon carbide, 8-10 parts of metal microfibers, 20-22 parts of calcium powder, 10-15 parts of water, 8-10 parts of water reducer and 2-3 parts of defoaming agent.
[0020] Furthermore, the defoaming agent is NXZ defoaming agent.
[0021] A method for preparing low-energy-consumption, high-strength, high-toughness soft porcelain, used to prepare the above-mentioned low-energy-consumption, high-strength, high-toughness soft porcelain, comprising the following steps:
[0022] A. According to the formula of the bottom slurry, the defoamer, water reducer and water are mixed evenly to obtain a first mixed material; the cement, quartz sand, silicon carbide and calcium powder are mixed evenly to obtain a first intermediate material; the emulsion is added to the first intermediate material and mixed evenly, and then the first mixed material is added and mixed evenly to obtain a bottom slurry;
[0023] B. According to the formula of the surface slurry, the defoamer, water reducer and water are mixed evenly to obtain a second mixed material; the cement, quartz sand, silicon carbide, metal microfiber and calcium powder are mixed evenly to obtain a second intermediate material; the emulsion is added to the second intermediate material and mixed evenly, and then the second mixed material is added and mixed evenly to obtain a surface slurry;
[0024] C. Inject the surface layer slurry into the mold to form the surface layer; lay the glass fiber mesh on the surface of the surface layer to form the middle layer; inject the bottom layer slurry on the surface of the middle layer to form the bottom layer, and cure it at 110-120°C for 50-55 minutes to obtain low-energy consumption, high-strength and high-toughness soft porcelain.
[0025] The technical solution provided by the embodiments of the present application may have the following beneficial effects:
[0026] 1. Through the cement, emulsion, quartz sand, calcium powder and silicon carbide in the bottom slurry, and the cement, emulsion, quartz sand, calcium powder, silicon carbide and metal microfiber in the surface slurry, the bottom slurry and the surface slurry have high strength and flexibility, so that the surface layer and the bottom layer have high strength and flexibility, thereby improving the strength and toughness of the soft porcelain. In addition, since the surface layer is in direct contact with the outside, its strength requirements are higher. Therefore, in this technical solution, the amount of quartz sand added in the surface slurry is higher than that in the bottom slurry to ensure the performance of the soft porcelain.
[0027] 2. In order to ensure the heat conduction efficiency of the heat energy source through the bottom layer and then to the middle layer and the surface layer, the technical solution specifically makes the addition amount of silicon carbide in the bottom layer slurry be 12 to 20 parts, and the addition amount of silicon carbide in the surface layer slurry be 5 to 10 parts, that is, the addition amount of silicon carbide in the bottom layer slurry is greater than the addition amount of silicon carbide in the surface layer slurry, which is beneficial to match the heat conduction efficiency of the bottom layer with the heat conduction efficiency of the surface layer, thereby reducing the loss of heat energy and achieving efficient heat energy conduction, making the curing temperature of the soft porcelain as low as 110 to 120°C, and the curing time as low as 50 to 55 minutes, realizing rapid low-temperature curing. Compared with the existing curing temperature of more than 150°C and the curing time of 60 to 90 minutes, it greatly reduces the production energy consumption of soft porcelain and realizes green production; at the same time, rapid low-temperature curing is also beneficial to avoid deformation of soft porcelain caused by excessively high curing temperature, resulting in reduced flexibility.
[0028] 3. The technical solution sets a glass fiber mesh as an intermediate layer between the bottom layer and the surface layer. Specifically, the glass fiber mesh is woven from glass fiber yarns and has high strength. When the glass fiber mesh is applied to the soft porcelain structure, it can significantly improve the overall strength of the soft porcelain, so that the soft porcelain material can withstand greater pressure and impact force, and reduce the risk of cracking and deformation. At the same time, the glass fiber mesh has excellent flexibility and plasticity, and can adapt to various complex building surfaces to form a smooth and seamless decorative effect, ensuring its decorativeness. Therefore, the technical solution optimizes the soft porcelain structure by setting an intermediate layer between the bottom layer and the surface layer, and combines the innovation of the bottom layer slurry and the surface layer slurry formula to make the soft porcelain have high strength and high flexibility, so that it can not only adapt to complex building surfaces, ensure the firmness of adhesion and the flatness after adhesion, but also withstand certain external forces and pressures, and is not easy to break or break, ensuring its use function. DETAILED DESCRIPTION
[0029] The technical solution provides a low-energy consumption, high-strength, high-toughness soft porcelain, comprising a bottom layer, an intermediate layer, and a surface layer arranged in sequence from bottom to top; the bottom layer is obtained by solidifying the bottom layer slurry, the intermediate layer is a glass fiber mesh, and the surface layer is obtained by solidifying the surface layer slurry;
[0030] Calculated by weight, the base slurry includes 3 to 5 parts of cement, 8 to 10 parts of emulsion, 45 to 53 parts of quartz sand, 12 to 20 parts of silicon carbide, 20 to 22 parts of calcium powder, 10 to 15 parts of water and 8 to 10 parts of water reducing agent;
[0031] Calculated by mass, the surface layer slurry includes 3-5 parts of cement, 8-10 parts of emulsion, 55-60 parts of quartz sand, 5-10 parts of silicon carbide, 6-12 parts of metal microfibers, 20-22 parts of calcium powder, 10-15 parts of water and 8-10 parts of water reducing agent.
[0032] In order to overcome the technical problems of high energy consumption of soft porcelain in the prior art and difficulty in taking into account high strength and high flexibility at the same time, the present technical solution proposes a low-energy consumption, high-strength and high-toughness soft porcelain. By optimizing the soft porcelain structure and the bottom slurry and the surface slurry, the curing temperature is reduced to 110-120°C, the curing time is reduced to 50-55°C, and it has high flexibility and strength, so that the soft porcelain can take into account low energy consumption, high strength and high flexibility at the same time to meet actual usage needs.
[0033] Specifically, the raw materials in the bottom slurry and the surface slurry in the technical solution include cement, emulsion, quartz sand, calcium powder and silicon carbide. Among them, cement adheres to the surface of quartz sand to wrap and bond the quartz sand, so that the bottom slurry and the surface slurry are bonded to form a whole, ensuring the strength of the bottom slurry and the surface slurry; the emulsion has good flexibility, so that the bottom slurry and the surface slurry have a certain strength, and can also maintain its unique softness, so that the soft porcelain is easy to construct and can adapt to various complex building surfaces; calcium powder can enhance the stability of the bottom slurry and the surface slurry, and prevent the bottom slurry obtained by curing the bottom slurry and the surface layer obtained by curing the surface slurry from cracking and deformation during use, thereby improving the density and overall performance of the bottom slurry and the surface slurry; silicon carbide has excellent mechanical strength, giving the bottom slurry and the surface slurry high strength. In addition, the raw materials of the surface slurry also include metal microfibers. Due to their micron-level lateral dimensions and continuous distribution of metal materials, the metal microfibers have good bending resistance and fatigue resistance under the action of external forces. When external force acts on the metal microfibers, the fibers can resist the external force, thereby reducing the impact of the external force on the reinforcement, making it more flexible and giving the surface slurry high flexibility.
[0034] Therefore, in the technical solution, the cement, emulsion, quartz sand, calcium powder and silicon carbide in the bottom slurry and the cement, emulsion, quartz sand, calcium powder, silicon carbide and metal microfiber in the surface slurry are used to make the bottom slurry and the surface slurry have high strength and flexibility, so that the surface layer and the bottom layer have high strength and flexibility, thereby improving the strength and toughness of the soft porcelain. In addition, since the surface layer is in direct contact with the outside, its strength requirements are higher. Therefore, in the technical solution, the amount of quartz sand added in the surface slurry is higher than that in the bottom slurry, so as to ensure the performance of the soft porcelain.
[0035] At the same time, the emulsion in the technical solution can also effectively resist the erosion of water, and prevent the soft porcelain from turning white due to water absorption during use. In addition, the technical solution uses the characteristics of calcium powder to improve the fluidity and plasticity of the bottom slurry and the surface slurry, making it easier for the soft porcelain to be molded into various shapes during processing, which is conducive to improving the processing efficiency of soft porcelain and reducing the processing difficulty.
[0036] Although the strength and toughness of soft porcelain can be effectively improved by optimizing the formula of the bottom slurry and the surface slurry, the overall flexibility and strength of the soft porcelain are still insufficient if the strength and toughness of the soft porcelain are optimized only by the formula of the bottom slurry and the surface slurry. Therefore, the technical solution sets a glass fiber mesh as an intermediate layer between the bottom layer and the surface layer. Specifically, the glass fiber mesh is woven from glass fiber yarns, which has high strength. When the glass fiber mesh is applied to the soft porcelain structure, it can significantly improve the overall strength of the soft porcelain, so that the soft porcelain material can withstand greater pressure and impact force, and reduce the risk of cracking and deformation. At the same time, the glass fiber mesh has excellent flexibility and plasticity, and can adapt to various complex building surfaces to form a smooth and seamless decorative effect, ensuring its decorativeness. Therefore, this technical solution optimizes the soft porcelain structure by setting an intermediate layer between the base layer and the surface layer, and combines the innovation of the base layer slurry and the surface layer slurry formula to make the soft porcelain have high strength and high flexibility, so that it can not only adapt to complex building surfaces, ensure the firmness of adhesion and the flatness after adhesion, but also withstand certain external forces and pressures, and is not prone to breakage or damage, thereby ensuring its functionality.
[0037] Furthermore, in the prior art, the thermally conductive raw materials in the base slurry and the surface slurry are generally quartz sand and silicon micropowder, and the thermal conductivity of quartz sand is 3.1-7.8W / (m·k), and the thermal conductivity of silicon micropowder is only 0.27W / (m·k). Both have poor thermal conductivity, which is not conducive to the low-temperature rapid curing of the base slurry and the surface slurry, resulting in high energy consumption. Therefore, the design of the thermal conductivity of the base slurry and the surface slurry in the present technical solution cannot be based on the above principle.
[0038] Therefore, in order to improve the thermal conductivity of the bottom slurry and the surface slurry, so that the soft porcelain can be quickly solidified at low temperature and achieve the purpose of energy saving and consumption reduction, the technical solution adds silicon carbide to both the bottom slurry and the surface slurry. The thermal conductivity of silicon carbide is 83.6W / (m·k), which greatly improves the heat conduction efficiency. At the same time, since the surface slurry also includes metal microfibers with good thermal conductivity, only silicon carbide is added to the bottom slurry, and the bottom layer obtained by the bottom slurry is in direct contact with the heat source. In order to ensure the heat conduction efficiency of the heat energy source through the bottom layer and then to the middle layer and the surface layer, the technical solution specifically makes the addition amount of silicon carbide in the bottom layer slurry be 12 to 20 parts, and the addition amount of silicon carbide in the surface layer slurry be 5 to 10 parts, that is, the addition amount of silicon carbide in the bottom layer slurry is greater than the addition amount of silicon carbide in the surface layer slurry, which is beneficial to match the heat conduction efficiency of the bottom layer with the heat conduction efficiency of the surface layer, thereby reducing the loss of heat energy and achieving efficient heat energy conduction, making the curing temperature of the soft porcelain as low as 110 to 120°C, and the curing time as low as 50 to 55 minutes, realizing rapid low-temperature curing. Compared with the existing curing temperature of more than 150°C and the curing time of 60 to 90 minutes, the production energy consumption of soft porcelain is greatly reduced, realizing green production; at the same time, rapid low-temperature curing is also beneficial to avoid deformation of soft porcelain caused by excessively high curing temperature, resulting in reduced flexibility.
[0039] Preferably, the water reducing agents in the base slurry and the surface slurry are both polycarboxylic acid water reducing agents.
[0040] In a preferred embodiment of the present technical solution, both the bottom slurry and the surface slurry contain polycarboxylic acid water reducer, which can reduce water consumption on the one hand, and help improve the strength and flexibility of soft porcelain on the other hand, ensuring product performance.
[0041] It is further described that the diameter of the metal microfiber is 1 to 30 μm and the length is 0.3 to 0.5 cm.
[0042] When the diameter of the metal microfiber is larger, it is more difficult to bend, resulting in the surface slurry not being easy to be slurried and molded; and when the length of the metal microfiber is too long, it will affect the stirring performance of the mixer, resulting in the surface slurry not being easy to mix evenly; when the length of the metal microfiber is too short, its toughening effect is limited. Therefore, in a preferred embodiment of the present technical solution, the diameter of the metal microfiber is limited to 1-30 μm, and the length is limited to 0.3-0.5 cm, to ensure the fluidity of the surface slurry, to make it mix evenly, and to ensure the relevant properties of the surface slurry.
[0043] It is further specified that the metal microfibers include any one of stainless steel microfibers, silver microfibers and aluminum microfibers.
[0044] Since stainless steel microfibers, silver microfibers and aluminum microfibers all have good thermal conductivity and high flexibility, the technical solution limits the metal microfibers to any one of stainless steel microfibers, silver microfibers and aluminum microfibers to ensure the performance of the surface slurry.
[0045] Preferably, the metal microfibers are stainless steel microfibers, so as to improve the thermal conductivity and flexibility of the soft porcelain at a lower cost.
[0046] It is further explained that the mesh size of the quartz sand in the base slurry and the surface slurry is 60-325 meshes, the mesh size of the silicon carbide is 70-120 meshes, and the mesh size of the calcium powder is 380-400 meshes.
[0047] In a preferred embodiment of the present technical solution, by optimizing the mesh size of quartz sand, it is helpful to ensure a reasonable particle size gradation, increase the density of the bottom layer slurry and the surface layer slurry, and ensure the performance of the soft porcelain.
[0048] Furthermore, when the mesh number of silicon carbide is too large, its particles are too coarse, resulting in a rough and granular surface of the obtained soft porcelain product; when the mesh number of silicon carbide is too small, its thermal conductivity becomes poor.
[0049] Furthermore, by limiting the mesh size of calcium powder, its filling performance as a filler is ensured, thereby ensuring the quality stability and consistency of soft porcelain products.
[0050] It is further explained that the emulsions in the base slurry and the surface slurry both include at least one of silicone-acrylic emulsion, pure acrylic emulsion and styrene-acrylic emulsion.
[0051] Pure acrylic emulsion has good weather resistance, aging resistance and color and gloss retention; styrene acrylic emulsion is a milky white liquid with good adhesion and good water resistance, oil resistance, heat resistance and aging resistance; silicone acrylic emulsion has good aging resistance and good flexibility and strength. Therefore, in a preferred embodiment of the present technical solution, the emulsions in the bottom slurry and the surface slurry include at least one of silicone acrylic emulsion, pure acrylic emulsion and styrene acrylic emulsion to ensure the performance of soft porcelain.
[0052] Preferably, the emulsions in the base slurry and the surface slurry are both silicone-acrylic emulsions.
[0053] It is further explained that the cement in the base layer slurry and the surface layer slurry is white PO 42.5R cement.
[0054] Since white P.O42.5R cement has the advantages of excellent durability, impermeability and high strength, and since the color of white P.O42.5R cement is pure white, it is conducive to ensuring the original color and pattern of soft porcelain, making soft porcelain more suitable for use occasions with high requirements for purity and aesthetics. Therefore, in a preferred embodiment of the present technical solution, the cement in both the bottom slurry and the surface slurry is white P.O42.5R cement to ensure the strength of soft porcelain and make it suitable for high-end application fields.
[0055] Further description, the thickness of the bottom layer is 0.5-1 mm, the thickness of the middle layer is 0.2-0.5 mm, and the thickness of the surface layer is 2-3 mm.
[0056] Since the performance of soft porcelain mainly depends on the surface layer, in a preferred embodiment of the present technical solution, the thickness of the surface layer is thicker than the bottom layer and the middle layer, and the thickness of the bottom layer, the middle layer and the surface layer is limited, which, on the one hand, ensures that the total thickness of the soft porcelain is moderate, with lower production and transportation costs; on the other hand, it is conducive to ensuring the performance of the soft porcelain.
[0057] It is further explained that both the bottom slurry and the surface slurry further include a defoaming agent;
[0058] Calculated by weight, the base slurry includes 3-5 parts of cement, 8-10 parts of emulsion, 45-53 parts of quartz sand, 15-18 parts of silicon carbide, 20-22 parts of calcium powder, 10-15 parts of water, 8-10 parts of water reducer and 2-3 parts of defoamer;
[0059] Calculated by mass, the surface layer slurry includes 3-5 parts of cement, 8-10 parts of emulsion, 55-60 parts of quartz sand, 8-10 parts of silicon carbide, 8-10 parts of metal microfibers, 20-22 parts of calcium powder, 10-15 parts of water, 8-10 parts of water reducer and 2-3 parts of defoaming agent.
[0060] In a preferred embodiment of the present technical solution, defoamers are added to both the bottom slurry and the surface slurry to eliminate bubbles in the bottom slurry and the surface slurry, thereby increasing the density of the soft porcelain product and ensuring its appearance. At the same time, further optimizing the bottom slurry and the surface slurry is conducive to achieving better performance of the bottom slurry and the surface slurry, further ensuring the performance of the soft porcelain.
[0061] It is further specified that the defoamer is NXZ defoamer.
[0062] In a preferred embodiment of the present technical solution, the defoamer is NXZ defoamer (i.e., mineral oil hydrophobic fumed silica and metal soap defoamer). NXZ defoamer not only has excellent defoaming and foam suppression effects, but also has good compatibility with the slurry system of the present technical solution, ensuring the performance of the bottom slurry and the surface slurry.
[0063] A method for preparing low-energy-consumption, high-strength, high-toughness soft porcelain, used to prepare the above-mentioned low-energy-consumption, high-strength, high-toughness soft porcelain, comprising the following steps:
[0064] A. According to the formula of the bottom slurry, the defoamer, water reducer and water are mixed evenly to obtain a first mixed material; the cement, quartz sand, silicon carbide and calcium powder are mixed evenly to obtain a first intermediate material; the emulsion is added to the first intermediate material and mixed evenly, and then the first mixed material is added and mixed evenly to obtain a bottom slurry;
[0065] B. According to the formula of the surface slurry, the defoamer, water reducer and water are mixed evenly to obtain a second mixed material; the cement, quartz sand, silicon carbide, metal microfiber and calcium powder are mixed evenly to obtain a second intermediate material; the emulsion is added to the second intermediate material and mixed evenly, and then the second mixed material is added and mixed evenly to obtain a surface slurry;
[0066] C. Inject the surface layer slurry into the mold to form the surface layer; lay the glass fiber mesh on the surface of the surface layer to form the middle layer; inject the bottom layer slurry on the surface of the middle layer to form the bottom layer, and cure it at 110-120°C for 50-55 minutes to obtain low-energy consumption, high-strength and high-toughness soft porcelain.
[0067] The technical solution also proposes a method for preparing soft porcelain with low energy consumption, high strength and high toughness. The method has simple steps and strong operability, which is conducive to ensuring the relevant properties of the soft porcelain during the preparation process.
[0068] Specifically, in the present technical solution, when preparing the base slurry and the surface slurry, water is first used to mix the water reducer and the defoamer to ensure the uniformity of the dispersion and stirring of the water reducer and the defoamer, so as to avoid the uneven dispersion of the water reducer and the defoamer and the influence on the performance of the soft porcelain.
[0069] Preferably, in step C, the inner wall of the mold has a finishing texture.
[0070] In a preferred embodiment of the present technical solution, by limiting the inner wall of the mold to have a finishing texture, a certain texture effect can be produced on the surface of the soft porcelain, thereby improving the appearance texture of the soft porcelain and increasing the added value of the product.
[0071] Preferably, in step C, the tensile strength of the low-energy consumption, high-strength and high-toughness soft porcelain is greater than 9.3 MPa.
[0072] In a preferred embodiment of the present technical solution, the tensile strength of the soft porcelain is greater than 9.3 MPa, and the surface is free of cracks, which is beneficial for reducing the energy consumption of the soft porcelain while having high strength and high flexibility to meet the use requirements.
[0073] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0074] Performance Testing:
[0075] Flexibility test: refer to JC / T 2219-2014 standard, observe whether there are cracks or fractures at the bending part of the test piece surface, where the diameter of the arc mold is 100mm.
[0076] Tensile strength test: stick the soft porcelain and the cured specimen together with a high-strength adhesive, cut the soft porcelain to the base along the fixture to make the test area (40×40) mm, install the specimen with the tensile fixture on the testing machine, keep the center line of the specimen surface in the vertical direction and the center of the testing machine fixture in line, stretch at a speed of (5±1) mm / min until the soft porcelain is destroyed, record the maximum tensile force when the soft porcelain is destroyed, and calculate the tensile strength of the soft porcelain according to σ=F / (a×b).
[0077] Example Group
[0078] Example 1
[0079] A. According to the formula of the bottom slurry, 2 parts of NXZ defoamer, 8 parts of polycarboxylate water reducer and 15 parts of water are mixed evenly to obtain a first mixture; 5 parts of white PO 42.5R cement, 50 parts of 60-mesh quartz sand, 15 parts of 70-mesh silicon carbide and 20 parts of 380-mesh calcium powder are mixed evenly to obtain a first intermediate material; 10 parts of silicone-acrylic emulsion are added to the first intermediate material and mixed evenly, and then the first mixture is added and mixed evenly to obtain a bottom slurry;
[0080] B. According to the formula of the surface slurry, 2 parts of NXZ defoamer, 8 parts of polycarboxylic acid water reducer and 15 parts of water are mixed evenly to obtain a second mixture; 5 parts of white PO 42.5R cement, 55 parts of 60-mesh quartz sand, 8 parts of 70-mesh silicon carbide, 10 parts of stainless steel microfibers with a diameter of 25 μm and a length of 0.3 cm and 20 parts of 380-mesh calcium powder are mixed evenly to obtain a second intermediate material; 10 parts of silicone acrylic emulsion are added to the second intermediate material and mixed evenly, and then the second mixture is added and mixed evenly to obtain a surface slurry;
[0081] C. Inject the surface layer slurry into the mold to form a surface layer with a thickness of 2 mm; lay a glass fiber mesh on the surface of the 2 mm thick surface layer to form a middle layer with a thickness of 0.2 mm; inject the bottom layer slurry on the surface of the 0.2 mm thick middle layer to form a bottom layer with a thickness of 0.5 mm, and cure it at 110°C for 53 minutes to obtain low-energy consumption, high-strength and high-toughness soft porcelain.
[0082] Example 2
[0083] A. According to the formula of the bottom slurry, 3 parts of NXZ defoamer, 10 parts of polycarboxylic acid water reducer and 10 parts of water are mixed evenly to obtain a first mixture; 3 parts of white PO 42.5R cement, 45 parts of 325 mesh quartz sand, 12 parts of 120 mesh silicon carbide and 22 parts of 400 mesh calcium powder are mixed evenly to obtain a first intermediate material; 10 parts of pure acrylic emulsion are added to the first intermediate material and mixed evenly, and then the first mixture is added and mixed evenly to obtain a bottom slurry;
[0084] B. According to the formula of the surface slurry, 3 parts of NXZ defoamer, 10 parts of polycarboxylic acid water reducer and 10 parts of water are mixed evenly to obtain a second mixture; 3 parts of white PO 42.5R cement, 60 parts of 325 mesh quartz sand, 5 parts of 120 mesh silicon carbide, 6 parts of silver microfibers with a diameter of 5 μm and a length of 0.4 cm and 22 parts of 400 mesh calcium powder are mixed evenly to obtain a second intermediate material; 10 parts of pure acrylic emulsion are added to the second intermediate material and mixed evenly, and then the second mixture is added and mixed evenly to obtain a surface slurry;
[0085] C. Inject the surface layer slurry into the mold to form a surface layer with a thickness of 3 mm; lay a glass fiber mesh on the surface of the 3 mm thick surface layer to form a middle layer with a thickness of 0.4 mm; inject the bottom layer slurry on the surface of the 0.4 mm thick middle layer to form a bottom layer with a thickness of 0.8 mm, and cure it at 120°C for 50 minutes to obtain low-energy consumption, high-strength and high-toughness soft porcelain.
[0086] Example 3
[0087] A. According to the formula of the bottom slurry, 3 parts of NXZ defoamer, 9 parts of polycarboxylic acid water reducer and 13 parts of water are mixed evenly to obtain a first mixed material; 4 parts of white PO 42.5R cement, 53 parts of 200-mesh quartz sand, 20 parts of 90-mesh silicon carbide and 21 parts of 390-mesh calcium powder are mixed evenly to obtain a first intermediate material; 9 parts of styrene-acrylic emulsion are added to the first intermediate material and mixed evenly, and then the first mixed material is added and mixed evenly to obtain a bottom slurry;
[0088] B. According to the formula of the surface slurry, 3 parts of NXZ defoamer, 9 parts of polycarboxylic acid water reducer and 13 parts of water are mixed evenly to obtain a second mixture; 4 parts of white PO 42.5R cement, 58 parts of 200-mesh quartz sand, 10 parts of 90-mesh silicon carbide, 8 parts of aluminum microfibers with a diameter of 10 μm and a length of 0.5 cm and 21 parts of 390-mesh calcium powder are mixed evenly to obtain a second intermediate material; 9 parts of styrene-acrylic emulsion are added to the second intermediate material and mixed evenly, and then the second mixture is added and mixed evenly to obtain a surface slurry;
[0089] C. Inject the surface layer slurry into the mold to form a surface layer with a thickness of 2.5 mm; lay a glass fiber mesh on the surface of the 2.5 mm thick surface layer to form a middle layer with a thickness of 0.2 mm; inject the bottom layer slurry on the surface of the 0.2 mm thick middle layer to form a bottom layer with a thickness of 1 mm, and cure it at 150°C for 52 minutes to obtain low-energy consumption, high-strength and high-toughness soft porcelain.
[0090] Comparative group
[0091] Comparative Example 1
[0092] The preparation method and raw materials of Comparative Example 1 are the same as those of Example 1, except that no intermediate layer is provided in Comparative Example 1.
[0093] Comparative Example 2
[0094] The preparation method and raw materials of Comparative Example 2 are the same as those of Example 1, except that silicon carbide is not added to the base layer slurry and the surface layer slurry formula in Comparative Example 2.
[0095] Comparative Example 3
[0096] The preparation method and raw materials of Comparative Example 3 are the same as those of Example 1, except that stainless steel microfibers are not added to the surface layer slurry formula in Comparative Example 3.
[0097] The soft porcelain was prepared by the preparation methods in the above embodiment and comparative example respectively, and the obtained soft porcelain was tested for flexibility, tensile strength and compressive strength. The results are shown in Table 1 below.
[0098] Table 1 Test results of relevant properties of soft porcelain
[0099] Experiment number Tensile strength(MPa) Flexibility Example 1 9.46 No cracks Example 2 9.42 No cracks Example 3 9.31 No cracks Comparative Example 1 / fracture Comparative Example 2 / / Comparative Example 3 8.12 There are tiny cracks
[0100] From the performance test results in Table 1, it can be seen that the soft porcelain prepared by the technical solution is a low-energy-consumption, high-strength and high-toughness soft porcelain, whose tensile strength is greater than 9.3MPa and has no cracks on the surface, which is beneficial to having high strength and high flexibility while reducing the energy consumption of the soft porcelain to meet the use requirements.
[0101] In Comparative Example 1, since no intermediate layer is provided, the strength and flexibility of the soft porcelain are reduced, and even broken.
[0102] In Comparative Example 2, since silicon carbide was not added to the base slurry and the surface slurry formula, the base slurry and the surface slurry could not be completely cured, and soft porcelain could not be obtained.
[0103] In Comparative Example 3, since stainless steel microfibers were not added to the surface layer slurry formula, the curing degree of the surface layer was slightly poor, which reduced the strength and flexibility of the soft porcelain. In addition, since the stainless steel microfibers also affected the flexibility of the surface layer, the flexibility of the soft porcelain was further reduced.
[0104] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.
Claims
1. A low-energy-consumption, high-strength, high-toughness soft porcelain, characterized in that: It comprises a bottom layer, an intermediate layer and a surface layer arranged in sequence from bottom to top; the bottom layer is obtained by solidifying the bottom layer slurry, the intermediate layer is a glass fiber mesh, and the surface layer is obtained by solidifying the surface layer slurry; Calculated by weight, the base slurry includes 3 to 5 parts of cement, 8 to 10 parts of emulsion, 45 to 53 parts of quartz sand, 12 to 20 parts of silicon carbide, 20 to 22 parts of calcium powder, 10 to 15 parts of water and 8 to 10 parts of water reducing agent; Calculated by mass, the surface layer slurry includes 3-5 parts of cement, 8-10 parts of emulsion, 55-60 parts of quartz sand, 5-10 parts of silicon carbide, 6-12 parts of metal microfibers, 20-22 parts of calcium powder, 10-15 parts of water and 8-10 parts of water reducing agent.
2. A low-energy-consumption, high-strength, high-toughness soft porcelain according to claim 1, characterized in that: The metal microfiber has a diameter of 1 to 30 μm and a length of 0.3 to 0.5 cm.
3. The low-energy-consumption, high-strength, high-toughness soft porcelain according to claim 1, characterized in that: The metal microfibers include any one of stainless steel microfibers, silver microfibers and aluminum microfibers.
4. The low-energy-consumption, high-strength, high-toughness soft porcelain according to claim 1, characterized in that: The mesh numbers of the quartz sand in the bottom layer slurry and the surface layer slurry are both 60-325 meshes, the mesh numbers of the silicon carbide are both 70-120 meshes, and the mesh numbers of the calcium powder are both 380-400 meshes.
5. The low-energy-consumption, high-strength, high-toughness soft porcelain according to claim 1, characterized in that: The emulsions in the base slurry and the surface slurry both include at least one of silicone-acrylic emulsion, pure acrylic emulsion and styrene-acrylic emulsion.
6. The low-energy-consumption, high-strength, high-toughness soft porcelain according to claim 1, characterized in that: The cement in the base layer slurry and the surface layer slurry is white PO 42.5R cement.
7. The low-energy-consumption, high-strength, high-toughness soft porcelain according to claim 1, characterized in that: The thickness of the bottom layer is 0.5-1 mm, the thickness of the middle layer is 0.2-0.5 mm, and the thickness of the surface layer is 2-3 mm.
8. The low-energy-consumption, high-strength, high-toughness soft porcelain according to claim 1, characterized in that: The bottom layer slurry and the surface layer slurry both further include a defoaming agent; Calculated by weight, the base slurry includes 3-5 parts of cement, 8-10 parts of emulsion, 45-53 parts of quartz sand, 15-18 parts of silicon carbide, 20-22 parts of calcium powder, 10-15 parts of water, 8-10 parts of water reducer and 2-3 parts of defoamer; Calculated by mass, the surface layer slurry includes 3-5 parts of cement, 8-10 parts of emulsion, 55-60 parts of quartz sand, 8-10 parts of silicon carbide, 8-10 parts of metal microfibers, 20-22 parts of calcium powder, 10-15 parts of water, 8-10 parts of water reducer and 2-3 parts of defoaming agent.
9. The low-energy-consumption, high-strength, high-toughness soft porcelain according to claim 8, characterized in that: The defoamer is NXZ defoamer.
10. A method for preparing low-energy-consumption, high-strength and high-toughness soft porcelain, characterized in that: The method for preparing the low-energy-consumption, high-strength and high-toughness soft porcelain as claimed in any one of claims 8 to 9 comprises the following steps: A. According to the formula of the bottom slurry, the defoamer, water reducer and water are mixed evenly to obtain a first mixed material; the cement, quartz sand, silicon carbide and calcium powder are mixed evenly to obtain a first intermediate material; the emulsion is added to the first intermediate material and mixed evenly, and then the first mixed material is added and mixed evenly to obtain a bottom slurry; B. According to the formula of the surface slurry, the defoamer, water reducer and water are mixed evenly to obtain a second mixed material; the cement, quartz sand, silicon carbide, metal microfiber and calcium powder are mixed evenly to obtain a second intermediate material; the emulsion is added to the second intermediate material and mixed evenly, and then the second mixed material is added and mixed evenly to obtain a surface slurry; C. Inject the surface layer slurry into the mold to form the surface layer; lay the glass fiber mesh on the surface of the surface layer to form the middle layer; inject the bottom layer slurry on the surface of the middle layer to form the bottom layer, and cure it at 110-120°C for 50-55 minutes to obtain low-energy consumption, high-strength and high-toughness soft porcelain.
Citation Information
Patent Citations
Porcelain-like coating and flexible stone-like tapestry brick
CN109626868A