Building dry-mixed mortar composition

By combining aggregates and additives, the problem of deterioration of thixotropy of dry powder mortar caused by cellulose ether is solved, the mechanical properties and construction properties of the mortar are improved, and the effect of not being easy to adhere to the tool is achieved.

CN118955076AInactive Publication Date: 2024-11-15WUHAN PINTAI NEW BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411086341.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The addition of cellulose ether in existing dry powder mortars leads to poor thixotropy, resulting in increased construction difficulty and decreased mechanical properties.

Method used

Using composite aggregates and additives, including fly ash, iron tailings, zeolite waste residue, vitrified microbeads, hemihydrate gypsum, polypropylene fiber, styrene methyl methacrylate and cellulose ether and other components , and vitrified microbeads and phosphoric acid-acidized zeolite waste residue are modified by silane coupling agent to optimize the interface binding force and dispersion of the mortar, and improve the thixotropy and mechanical properties.

Benefits of technology

It achieves the improvement of the thixotropy of the mortar while maintaining excellent mechanical properties, avoiding adhesion to the operating tool, and improving the overall performance of the mortar, including compressive strength and crack resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004985282700000091
    Figure BDA0004985282700000091
  • Figure BDA0004985282700000101
    Figure BDA0004985282700000101
Patent Text Reader

Abstract

The invention belongs to the field of building materials, and relates to dry-mixed mortar, in particular to a building dry-mixed mortar composition. The composition comprises the following components in parts by weight: 50-80 parts of aggregate, 10-15 parts of admixture and 3-5 parts of auxiliaries, the aggregate comprises 10-15 wt% of fly ash, 10-15 wt% of iron tailings, 5-8 wt% of zeolite waste residues and glass beads, and the total weight of the aggregate is 100 wt%; the admixture comprises 10 to 20 weight percent of semi-hydrated gypsum, 0.3 to 0.6 weight percent of polypropylene fiber, 1 to 3 weight percent of styrene methyl methacrylate and cellulose ether, and the total weight of the admixture is 100 weight percent; and the auxiliary agent comprises 5-8 wt% of an alkaline activator, 2-4 wt% of a water reducing agent, 0.1-0.2 wt% of an air entraining agent and 0.3-0.5 wt% of a water repellent. By compounding the aggregates, the admixture and the additive, the thixotropic dry-mixed mortar has excellent mechanical properties and good thixotropy, so that the thixotropic dry-mixed mortar is not easy to adhere to an operation tool, and the technical problem that the thixotropy of the dry-mixed mortar becomes poor due to doping of cellulose ether is properly solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of building materials and relates to a dry-mix mortar, and in particular to a building dry-mix mortar composition. Background Art

[0002] Dry-mixed mortar, also known as dry-mixed mortar or dry-mixed mortar, refers to a granular or powdered mixture of aggregates and additives that have been dried and sieved and mixed in a certain proportion. my country's research on dry-mixed mortar began in the 1980s. The first dry-mixed mortar products were mainly used for exterior wall insulation, mainly in the form of bonding mortar and plastering mortar. Dry-mixed mortar has the advantages of high production efficiency and stable product quality, and has developed rapidly in my country.

[0003] The main component for adjusting the application performance of mortar is to modify the mortar by mixing additives with different functions into the mortar. Among them, water-retaining thickener is one of the most important admixtures, and cellulose ether is the most common water-retaining thickener. Hydroxypropyl methylcellulose ether is a common cellulose ether and is now frequently used in the field of dry mortar.

[0004] However, hydroxypropyl methylcellulose ether, for example, will bring new problems after being added to dry-mix mortar: after adding hydroxypropyl methylcellulose ether, the thixotropy of the mortar viscosity will deteriorate. During field construction, the mortar and water will adhere to operating tools such as brick knives after mixing, which is not conducive to the smoothing of the wall surface and makes construction difficult. In this regard, some scholars have proposed that the thixotropy of dry-mix mortar can be increased by adding acetate starch to the mortar, and relevant experiments have verified this. However, under the conditions of freeze-thaw cycles, starch repeatedly absorbs water and dehydrates, and repeated volume changes will cause internal stress concentration in the mortar; at the same time, starch may also cause uneven hydration of other additives. Both of the above situations will lead to deterioration of the mechanical properties of the mortar, such as the compressive strength.

[0005] In summary, there is still no good solution in the existing technology to deal with the problem of poor thixotropy of dry-mixed mortar caused by adding cellulose ether to it, which often leads to new problems such as poor mechanical strength. Therefore, how to reconcile the positive and negative contributions of cellulose ether to dry-mixed mortar still needs to be solved. Summary of the invention

[0006] In order to ensure the positive effect of cellulose ether on dry-mix mortar while eliminating the technical problem of deterioration of thixotropy caused by cellulose ether as much as possible, the present application provides a building dry-mix mortar mixture.

[0007] In a first aspect, the present application provides a building dry mortar mixture, which adopts the following technical solution:

[0008] A building dry mortar composition comprises the following components in parts by weight:

[0009] 50-80 parts of aggregate, 10-15 parts of admixture, 3-5 parts of additives;

[0010] The aggregate, based on its own weight as 100wt%, includes 10-15wt% fly ash, 10-15wt% iron tailings, 5-8wt% zeolite waste slag, and also includes vitrified microspheres, and the vitrified microspheres are supplemented to 100wt%;

[0011] The admixture, based on its own weight as 100wt%, includes 10-20wt% of hemihydrate gypsum, 0.3-0.6wt% of polypropylene fiber, 1-3wt% of styrene methyl methacrylate, and also includes cellulose ether, and the cellulose ether is supplemented to 100wt%;

[0012] The additives, based on 100wt% of the aggregate weight, include 5-8wt% of alkaline activator, 2-4wt% of water reducer, 0.1-0.2wt% of air entraining agent, and 0.3-0.5wt% of water repellent.

[0013] In a specific embodiment, the glass microspheres are glass microspheres modified with a silane coupling agent; the preparation steps of the glass microspheres modified with a silane coupling agent are: dissolving the silane coupling agent in water at a volume ratio of 1:60 to 80, then spraying it onto the surface of the glass microspheres, and then drying it at 140 to 200°C.

[0014] In a specific embodiment, the cellulose ether is HPMC-20, the methoxy content of which is no more than 20%, the hydroxypropyl content is no more than 8%, and the ash content is no more than 1%.

[0015] In a specific embodiment, the zeolitic waste residue is zeolitic waste residue acidified with phosphoric acid.

[0016] In a specific embodiment, the alkaline activator includes any one of sodium sulfate or sodium silicate.

[0017] In a specific embodiment, the water reducing agent includes lignin sulfonate.

[0018] In a specific embodiment, the air entraining agent includes a soap-entraining agent.

[0019] In a specific embodiment, the water repellent comprises an alkyl sulfonate.

[0020] In a specific embodiment, the particle size of the vitrified microspheres is 0.5-1.5 mm, the surface vitrification rate is ≥92.4%, and the water absorption rate is 25-35%.

[0021] In a second aspect, the present application provides a method for forming a slurry from a dry-mix mortar composition, using the following technical solution:

[0022] A method for forming a slurry from a dry mortar composition comprises the following steps:

[0023] Aggregates, admixtures, water reducers, air entraining agents and water repellents are weighed by weight, dissolved in water to form a primary slurry with a moisture content of 10-20%; after stirring the primary slurry for 3-5 minutes, an alkaline activator is weighed by weight, added to the primary slurry, and stirred thoroughly to obtain a slurry.

[0024] The present application includes at least one of the following beneficial technical effects:

[0025] 1. The present application, by compounding various aggregates, admixtures and additives, has excellent mechanical properties and good thixotropy, making it difficult to adhere to operating tools, and properly optimizes the technical problem of poor thixotropy of dry mortar caused by doping with cellulose ether.

[0026] 2. The present application preferably utilizes silane coupling agent to modify the glass microspheres. After the glass microspheres are modified by silane coupling agent KH-550, the thixotropic index and mechanical properties of the mortar are improved by enhancing the interfacial bonding force between the glass microspheres and the mortar system and improving their dispersibility and wettability in the mortar.

[0027] 3. The present application preferably utilizes phosphoric acid to acidify zeolite waste slag. After phosphoric acid acidification, the surface properties, microstructure and interfacial bonding strength of the zeolite waste slag with the mortar matrix are improved, thereby improving the thixotropic index and mechanical properties of the mortar. DETAILED DESCRIPTION

[0028] The present application is described in further detail below.

[0029] The development of cellulose ether in dry-mix mortar is getting faster and faster, but the problems that come with it are also becoming more and more obvious, namely, the deterioration of thixotropy of mortar and the problem of adhesion to operating tools.

[0030] The applicant found that the deterioration of thixotropy is mainly because cellulose ether can increase the viscosity of the mortar in the traditional dry-mix mortar with sand or silicate cement as aggregate, making the mortar viscous, which is beneficial to prevent the mortar from stratification and segregation. However, it will also make the viscosity of the mortar not change significantly when subjected to shear force. The essence is that cellulose ether is a high-molecular water-soluble polymer with a long molecular chain. If it is added too much, it is easy to form a network structure, which limits the shear fluidity of the mortar. However, if the amount of cellulose ether is reduced for this reason, the positive effects brought by cellulose ether, such as reducing the amount of cement and the strength after hardening, will also be reduced, which is difficult to balance.

[0031] In response to this, the applicant improved the above problems through practical work experience and a large amount of existing technology summary.

[0032] First, the applicant abandoned the commonly used sand and silicate cement as aggregates, selected vitrified microspheres as the main aggregate, and then combined fly ash, iron tailings and zeolite waste slag to form a new aggregate; at the same time, semi-hydrated gypsum, polypropylene fiber, styrene methyl methacrylate, and cellulose ether were used as admixtures, assisted by auxiliary agents, and finally formed a building dry mortar composition of the present application.

[0033] The present application is further described below in conjunction with specific embodiments.

[0034] It should be noted that in the following examples, the cellulose ether is HPMC-20, the methoxy content is 20%, the hydroxypropyl content is 8%, the volatile content is 2%, and the ash content is 1%; the particle size of the vitrified microspheres is 0.5-1.5 mm, the surface vitrification rate is ≥92.4%, and the water absorption rate is 25-35%. The parameters of fly ash are: density 2.42 g / cm 3 ,45μm sieve residue is 21.4%, and loss on ignition is 2.4%.

[0035] Example 1

[0036] This embodiment provides a building dry mortar composition, which includes:

[0037] 5kg aggregate, 1kg admixture, 0.3kg additive.

[0038] The aggregate, based on its own weight as 100wt%, includes 10wt% fly ash, 10wt% iron tailings, 5wt% zeolite waste slag, and vitrified microspheres, and the vitrified microspheres are supplemented to 100wt%;

[0039] The admixture, based on its own weight as 100wt%, includes 10wt% of hemihydrate gypsum, 0.3wt% of polypropylene fiber, 1wt% of styrene methyl methacrylate, and cellulose ether, and the cellulose ether is supplemented to 100wt%;

[0040] The additives, based on 100wt% of the aggregate weight, include 5wt% of alkaline activator, 2wt% of water reducing agent, 0.1wt% of air entraining agent, and 0.3wt% of water repellent.

[0041] In this embodiment, the alkaline activator is sodium silicate, the water reducing agent is sodium lignin sulfonate, the air entraining agent is soap air entraining agent, the water repellent is sodium alkyl sulfonate, the particle size of the vitrified microspheres is 1 mm, the surface vitrification rate is ≥92.4%, and the water absorption rate is 30%; the particle size of the remaining components of the aggregate excluding the vitrified microspheres and the admixtures are all 100 to 200 mesh unless otherwise specified.

[0042] Example 2

[0043] This embodiment provides a building dry mortar composition, which includes:

[0044] 6.5kg aggregate, 1.3kg admixture, and 0.4kg additive.

[0045] The aggregate, based on its own weight as 100wt%, includes 12wt% fly ash, 13wt% iron tailings, 6wt% zeolite waste slag, and also includes vitrified microspheres, and the vitrified microspheres are supplemented to 100wt%;

[0046] The admixture, based on its own weight as 100wt%, includes 15wt% of hemihydrate gypsum, 0.5wt% of polypropylene fiber, 2wt% of styrene methyl methacrylate, and cellulose ether, and the cellulose ether is supplemented to 100wt%;

[0047] The additives, based on 100wt% of the aggregate weight, include 6wt% of alkaline activator, 3wt% of water reducer, 0.15wt% of air entraining agent, and 0.4wt% of water repellent.

[0048] In this embodiment, the alkaline activator is sodium glauber powder, the water reducing agent is sodium lignin sulfonate, the air entraining agent is soap air entraining agent, the water repellent is sodium alkyl sulfonate, the particle size of the vitrified microspheres is 1 mm, the surface vitrification rate is ≥92.4%, and the water absorption rate is 30%; the particle size of the remaining components of the aggregate excluding the vitrified microspheres and the admixtures are all 100 to 200 mesh unless otherwise specified.

[0049] Example 3

[0050] This embodiment provides a building dry mortar composition, which includes:

[0051] 8kg aggregate, 1.5kg admixture, 0.5kg additive.

[0052] The aggregate, based on its own weight as 100wt%, includes 15wt% fly ash, 15wt% iron tailings, 8wt% zeolite waste slag, and vitrified microspheres, and the vitrified microspheres are supplemented to 100wt%;

[0053] The admixture, based on its own weight as 100wt%, includes 20wt% of hemihydrate gypsum, 0.6wt% of polypropylene fiber, 3wt% of styrene methyl methacrylate, and cellulose ether, and the cellulose ether is supplemented to 100wt%;

[0054] The additives, based on 100wt% of the aggregate weight, include 8wt% of alkaline activator, 4wt% of water reducer, 0.2wt% of air entraining agent, and 0.5wt% of water repellent.

[0055] In this embodiment, the alkaline activator is sodium glauber powder, the water reducing agent is sodium lignin sulfonate, the air entraining agent is soap air entraining agent, the water repellent is sodium alkyl sulfonate, the particle size of the vitrified microspheres is 1 mm, the surface vitrification rate is ≥92.4%, and the water absorption rate is 30%; the particle size of the remaining components of the aggregate excluding the vitrified microspheres and the admixtures are all 100 to 200 mesh unless otherwise specified.

[0056] Example 4

[0057] The present application is based on the technical solution of Example 1, and further, the glass microspheres are glass microspheres modified by silane coupling agent KH-550. The modification method is: dispersing the silane coupling agent KH-550 in water at a volume ratio of 1:60, then spraying it on the surface of the glass microspheres, and then drying it at 200°C. The amounts and parameters of the remaining raw materials are the same as those in Example 1.

[0058] Example 5

[0059] The present application is based on the technical solution of Example 1, and further, the glass microspheres are glass microspheres of KH-550 modified with a silane coupling agent. The modification method is: dispersing the silane coupling agent KH-550 in water at a volume ratio of 1:70, then spraying it on the surface of the glass microspheres, and then drying it at 180°C. The amounts and parameters of the remaining raw materials are the same as those in Example 1.

[0060] Example 6

[0061] The present application is based on the technical solution of Example 1, and further, the glass microspheres are glass microspheres of KH-550 modified with a silane coupling agent. The modification method is: dispersing the silane coupling agent KH-550 in water at a volume ratio of 1:80, then spraying it on the surface of the glass microspheres, and then drying it at 140°C. The amounts and parameters of the remaining raw materials are the same as those in Example 1.

[0062] Example 7

[0063] The difference between this embodiment and embodiment 5 is that the zeolite waste residue is phosphoric acid-acidified zeolite waste residue. The acidification step is: immersing the acidified zeolite waste residue in a 1.5 mol / L phosphoric acid aqueous solution at 40° C. for 2 hours, and then filtering to obtain phosphoric acid-acidified zeolite waste residue.

[0064] Comparative Example 1

[0065] This comparative example is compared with Example 1, and the difference is that fly ash is lacking in the aggregate, and the missing weight is supplemented by vitrified microspheres.

[0066] Comparative Example 2

[0067] This comparative example is compared with Example 1, and the difference is that the aggregate lacks iron tailings, and the missing weight is supplemented by vitrified microspheres.

[0068] Comparative Example 3

[0069] Compared with Example 1, the difference between this comparative example and Example 1 is that the aggregate lacks zeolite waste slag, and the missing weight is supplemented by vitrified microspheres.

[0070] Comparative Example 4

[0071] This comparative example is compared with Example 1, except that the vitrified microspheres in the aggregate are replaced with an equal weight of silicate cement.

[0072] Comparative Example 5

[0073] This comparative example is compared with Example 1, and the difference is that the admixture lacks hemihydrate gypsum.

[0074] Comparative Example 6

[0075] This comparative example is compared with Example 1, and the difference is that the admixture lacks polypropylene fiber.

[0076] Comparative Example 7

[0077] This comparative example is compared with Example 1, and the difference is that styrene methyl methacrylate is missing in the admixture.

[0078] Performance testing

[0079] The above-mentioned embodiments and comparative examples are respectively prepared into slurries according to the following methods and are ready for molding: aggregate, admixture, water reducer, air entraining agent and water repellent are weighed and dissolved in water to form a slurry with a water content of 10-20%; after stirring the slurry for 3-5 minutes, an alkaline activator is weighed and added to the slurry, and a mixture is formed after sufficient stirring; then the mixture is fully vibrated and cured to form.

[0080] The performance test was carried out on each of the samples after curing and forming. The test indicators are as follows:

[0081] 1. Thixotropy test: This test was carried out according to the method described in the article "Preparation and Application of Modified Starch / Bentonite Dry Mix Mortar Admixtures" published by Yuan Ke in June 2011. After the mortar was prepared, it was left to stand for 1 minute for testing.

[0082] 2. Mechanical properties testing: The compressive and flexural strength tests of mortar are completed in accordance with GB / T 17671-2021 "Test method for strength of cement mortar (ISO method)".

[0083] The test results are shown in Table 1.

[0084] Table 1

[0085]

[0086]

[0087] Combining the test results in Table 1, we can see that:

[0088] 1. The samples of Examples 1 to 3 have excellent mechanical properties and good thixotropy, which makes them not easy to adhere to the operating tools, and properly optimizes the technical problem of poor thixotropy of dry mortar caused by doping with cellulose ether. At the same time, Examples 1 to 3 do not use large doses of organic matter as modifiers or fillers, such as starch, etc. The volume of the materials used changes little after absorbing water, and the problem of internal stress concentration caused by freeze-thaw cycles can be ignored. This is because the present application uses a combination of fly ash, iron tailings, zeolite waste slag and vitrified microspheres. These materials not only have excellent mechanical properties, but also provide a stable structural foundation for mortar. In particular, vitrified microspheres, which have moderate particle size, high surface vitrification rate and appropriate water absorption rate, help to improve the overall performance of mortar. At the same time, the addition of semi-hydrated gypsum can enhance the strength of mortar, and polypropylene fiber can increase the toughness and crack resistance of mortar. Styrene methyl methacrylate, as a polymer additive, can improve the adhesion and workability of mortar. Cellulose ether, as a water-retaining thickener, can effectively control the fluidity and thixotropy of mortar. In addition, alkaline activators (sodium silicate / sodium silicate) can activate some inert materials and improve the early strength of mortar. Water reducers (sodium lignin sulfonate) can reduce the water-cement ratio of mortar, increase strength and improve workability. Air entraining agents (soap air entraining agents) can introduce tiny bubbles to improve the frost resistance and durability of mortar. Water repellents (sodium alkyl sulfonates) can reduce the water absorption of mortar and improve its anti-seepage performance. The combination of the above components reduces the difficulty of construction and ensures the quality of construction.

[0089] 2. Combining Examples 4 to 6 with Example 1, it can be seen that after the glass microspheres are modified by the silane coupling agent, the thixotropic index and mechanical properties of the mortar are improved to a certain extent. This may be because the molecular structure of the silane coupling agent KH-550 contains an active primary amino functional group and three hydrolyzable ethoxy groups. This dual reactivity enables it to undergo a two-way chemical reaction with inorganic materials and organic polymers. In the process of modifying the glass microspheres, the ethoxy groups of KH-550 react with the inorganic groups on the surface of the glass microspheres to form chemical bonds, while the primary amino functional groups face outward and can react with the organic components in the mortar, thereby improving the dispersibility and wettability of the glass microspheres in the mortar. The modified glass microspheres are easier to disperse evenly in the mortar system, reducing the agglomeration and sedimentation of the mortar and improving the thixotropy of the mortar. In summary, after the silane coupling agent KH-550 modified the vitrified microspheres, the thixotropic index and mechanical properties of the mortar were improved by enhancing the interfacial bonding force between the vitrified microspheres and the mortar system and improving their dispersibility and wettability in the mortar.

[0090] 3. Combining Example 7 and Example 5, it can be seen that after the zeolite waste residue is phosphoric acidified, the thixotropic index and mechanical properties of the mortar are also improved to a certain extent. This may be because the surface of the zeolite waste residue will be covered with phosphoric acid during the phosphoric acidification process to form a phosphate layer, which changes the surface properties of the waste residue and makes it more hydrophilic, thereby improving the interaction with the water molecules in the mortar. At the same time, phosphoric acidification can dissolve some mineral components in the zeolite waste residue and release some ions and active groups. These ions and active groups can react chemically with other components in the mortar (such as cement hydration products) to form new chemical bonds. The new chemical bonding enhances the interfacial bonding force between the zeolite waste residue and the mortar matrix, allowing the zeolite waste residue to better play its reinforcing role. Third, phosphoric acidification can also make the microstructure of the zeolite waste residue more loose and porous, and these pore structures can absorb and store water, thereby further improving the thixotropy of the mortar. After phosphoric acid treatment, the interfacial bonding force between the zeolite waste residue and the mortar matrix is ​​enhanced, which enables the mortar to better transmit and disperse stress when subjected to external forces, thereby improving its mechanical properties. The improved microstructure of the zeolite waste residue also gives it higher strength, further enhancing the mechanical properties of the mortar. In addition, phosphoric acid treatment may also improve the mechanical properties of the mortar by affecting the hydration process and hardening process of the mortar. For example, phosphoric acid treatment may promote the hydration reaction of cement and generate more hydration products; or react with other components in the mortar to form more stable and stronger compounds.

[0091] The improvement of hydrophilicity makes it easier to disperse zeolite waste residue in mortar, reduces the agglomeration of particles, and thus improves the thixotropy of mortar.

[0092] 4. Combining Comparative Examples 1, 2, 3, 5 and Example 1, it can be seen that fly ash, iron tailings, and zeolite waste residue all contribute positively to the thixotropy of the mortar. The following is analyzed in combination with their respective possible mechanisms of action: ① The microbeads in fly ash can reduce the internal friction resistance of the mortar, improve the fluidity of the mortar, and help improve the construction performance of the mortar, making it easier to spread and smooth. Fly ash can also generate compounds such as hydrated calcium silicate and hydrated calcium aluminate with mortar, which can increase the hardness and strength of the mortar. The fine particles of fly ash can fill the voids in the mortar and increase the density of the mortar. This micro-aggregate effect can reduce the free water in the mortar, thereby improving its thixotropy and making the mortar less likely to flow or segregate during operation. ② The iron tailings sand particles are rough, sharp, and have many edges and corners. This particle shape characteristic can improve the shear fluidity and thixotropy of the mortar to a certain extent. Compared with the spherical particles of fly ash, its improvement effect may be different. ③ Zeolite residue has a large surface area and high porosity, which can increase the adhesion and stability of the mortar, thereby improving its thixotropy. The components in the zeolite residue may react with the components in the mortar to promote the hardening process of the mortar. This hardening reaction not only improves the strength of the mortar, but also helps to improve its thixotropy, because the hardened mortar is more stable and less likely to deform. At the same time, zeolite residue can control the distribution of particles in the mortar, reduce the gaps between particles, improve the density and impermeability of the mortar, and also help to improve the thixotropy of the mortar.

[0093] 5. Combining Comparative Example 4 and Example 1, it can be seen that the vitrified microspheres of the present application have more excellent mechanical properties in the mortar system of the present application than the commonly used silicate cement. This may be because the porous cavity structure inside the vitrified microspheres makes the vitrified microspheres light, but at the same time maintains a high strength, provides better skeleton support, thereby enhancing the strength of the entire mortar system, and also helps to reduce stress concentration in the mortar system, thereby improving its crack resistance; at the same time, the vitrified microspheres have good interface bonding with other components in the mortar system, and the material shrinkage rate is low, which can form a more compact structure and improve the overall mechanical properties of the mortar system.

[0094] 6. Combining Comparative Example 6 and Example 1, it can be seen that polypropylene fibers have a significant positive contribution to the mechanical properties of the mortar system of the present application. This may be because polypropylene fibers can be interspersed in the mortar to form a three-dimensional randomly distributed network structure, which can effectively prevent the expansion of cracks, just like a skeleton in the mortar, significantly enhancing the overall strength and durability of the mortar. At the same time, when subjected to force, polypropylene fibers can effectively disperse stress and avoid the formation and expansion of cracks. Studies have shown that after adding polypropylene fibers, the crack resistance of the mortar is significantly improved. The fiber diameter is very fine and the fiber spacing is small, so it has a significant crack-blocking effect, effectively inhibiting the generation and development of cracks in the mortar.

[0095] 7. It can be seen from Comparative Example 7 and Example 1 that styrene methyl methacrylate, as an organic additive, has a certain degree of positive effect on the thixotropy and mechanical properties of the mortar of the present application.

[0096] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and improved concepts of the present invention within the technical scope disclosed by the present invention, and they should be covered by the protection scope of the present invention.

Claims

1. A building dry mortar composition, It is characterized in that The composition comprises the following components in parts by weight: 50-80 parts of aggregate, 10-15 parts of admixture, 3-5 parts of additives; The aggregate, based on its own weight as 100wt%, includes 10-15wt% fly ash, 10-15wt% iron tailings, 5-8wt% zeolite waste slag, and also includes vitrified microspheres, and the vitrified microspheres are supplemented to 100wt%; The admixture, based on its own weight as 100wt%, includes 10-20wt% of hemihydrate gypsum, 0.3-0.6wt% of polypropylene fiber, 1-3wt% of styrene methyl methacrylate, and also includes cellulose ether, and the cellulose ether is supplemented to 100wt%; The additives, based on 100wt% of the aggregate weight, include 5-8wt% of alkaline activator, 2-4wt% of water reducer, 0.1-0.2wt% of air entraining agent, and 0.3-0.5wt% of water repellent.

2. A building dry mortar composition according to claim 1, Features: The glass microspheres are glass microspheres modified by a silane coupling agent. The preparation steps of the glass microspheres modified by a silane coupling agent are as follows: dissolving the silane coupling agent in water at a volume ratio of 1:60 to 80, then spraying the silane coupling agent onto the surface of the glass microspheres, and then drying at 140 to 200°C.

3. A building dry mortar composition according to claim 1, Features: The cellulose ether is HPMC-20, the methoxy content of which is no more than 20%, the hydroxypropyl content is no more than 8%, and the ash content is no more than 1%.

4. A building dry mortar composition according to claim 1, Features: The zeolite waste residue is the zeolite waste residue acidified with phosphoric acid.

5. A building dry mortar composition according to claim 1, Features: The alkaline activator includes any one of sodium sulfate or sodium silicate.

6. A building dry mortar composition according to claim 1, Features: The water reducing agent includes lignin sulfonate.

7. A building dry mortar composition according to claim 1, Features: The air entraining agent includes a soap-feeding air entraining agent.

8. A building dry mortar composition according to claim 1, Features: The water repellent includes alkyl sulfonates.

9. A building dry mortar composition according to claim 1, Features: The particle size of the vitrified microspheres is 0.5-1.5 mm, the surface vitrification rate is ≥92.4%, and the water absorption rate is 25-35%.

10. A method for forming a slurry from a dry-mix mortar composition according to any one of claims 1 to 8, It is characterized in that The steps include: Aggregates, admixtures, water reducers, air entraining agents and water repellents are weighed by weight, dissolved in water to form a primary slurry with a moisture content of 10-20%; after stirring the primary slurry for 3-5 minutes, an alkaline activator is weighed by weight, added to the primary slurry, and stirred thoroughly to obtain a slurry.