Ceramic fettling knife for electroceramic dry molding and preparation method of ceramic fettling knife

Through the feeding preparation method of one-time firing process and surface modification treatment, the problems of irregular appearance and high hardness in the molding process of ceramic blank refining knife are solved, and the low shrinkage, high precision and wear resistance of ceramic blank refining knife are achieved. , extends service life and reduces production costs.

CN118955105AActive Publication Date: 2024-11-15SINOMA JIANGXI ELECTRICAL PORCELAIN ELECTRIC CO LTD

Patent Information

Application Number
CN202411172758.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-15
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing ceramic blank repairing knife for electric porcelain dry forming has problems such as inability to produce batch and continuous production during the molding process. The appearance is irregular, the blade is not sharp, and the hardness of alumina ceramics during the grinding process leads to difficulty in grinding. Yamato is costly.

Method used

A single-firing process is used to prepare ceramic blank repair knives through feed preparation, injection molding, extraction and dewaxing and drying sintering. Spherical α-alumina powder and yttrium stabilized zirconium oxide powder of different particle sizes are used, and surface modification is carried out. The amount of organic plasticizer is reduced, the dispersion and sintering density of the powder in the organic binder are improved, and the size shrinkage rate is reduced.

Benefits of technology

It realizes low shrinkage, high precision, and low deformation of ceramic blank refining knives, regular appearance, sharp edge, good wear resistance, long service life, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure NE2OPUMCTRXQSBLJISJXFGVOFSZXNBS5WNCG5R2I
    Figure NE2OPUMCTRXQSBLJISJXFGVOFSZXNBS5WNCG5R2I
Patent Text Reader

Abstract

The invention belongs to the technical field of ceramic materials, and particularly relates to a ceramic fettling knife for electroceramic dry forming and a preparation method of the ceramic fettling knife. According to the preparation method of the ceramic fettling knife for electroceramic dry molding, spherical alpha alumina powder with different particle sizes is subjected to grain composition and then mixed with yttria-stabilized zirconia powder to serve as ceramic powder, and a surface modifier is adopted for carrying out surface modification treatment on the ceramic powder, so that the ceramic fettling knife for electroceramic dry molding is obtained. A feed is prepared from 88-92 wt.% of the ceramic powder subjected to surface modification treatment, 5-8 wt.% of an organic plasticizer and 0.5-5 wt.% of a sintering aid, injection molding, extraction dewaxing, drying and sintering are conducted in sequence, and the ceramic fettling knife is obtained. The ceramic fettling knife for dry forming of electroceramics is prepared by adopting a one-time sintering process, the size shrinkage rate is low, the appearance is regular, the blade is sharp, the difficulty of a grinding process is reduced, meanwhile, the ceramic fettling knife has good wear resistance and bending strength, and the service life is long.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic materials, and in particular relates to a ceramic trimming knife for dry-forming of electric porcelain and a preparation method thereof. Background Art

[0002] The ceramic trimming knife for dry forming of insulators is a ceramic cutting knife used in the trimming process of dry forming of insulators. When in use, the ceramic trimming knife is bonded and fixed to the metal handle and installed on the CNC trimming machine to cut the dry formed ceramic body to obtain insulator products of corresponding specifications. The ceramic body used for dry forming is generally pressed and formed by an isostatic press at a pressure of 110MPa. It has high hardness, high rigidity and strong cutting resistance, which puts forward high requirements on the appearance regularity, blade sharpness, wear resistance and other indicators of the ceramic trimming knife.

[0003] At present, the forming methods of ceramic trimming knives for dry forming of electric porcelain mainly adopt two methods: grouting forming and pressure forming. Both methods are to first fire the ceramic body, grind the blade, and then perform secondary firing. For example, in patent CN115784754A, secondary firing is adopted, and the grinding process is set between the biscuit firing process and the sintering process. By controlling the size shrinkage of the body after biscuit firing, the densification degree of the body is controlled, and the loss of the grinding wheel in the grinding process is reduced. The above production method has the problem that it cannot be produced in batches and continuously, and the ceramic trimming knives prepared at the same time also have the problems of irregular appearance and blunt blades.

[0004] In addition, patent CN109485393A discloses an alumina ceramic, which can be used for ceramic splitters. The invention greatly improves the bending strength, wear resistance and hardness of the alumina ceramic by adding spherical chromium oxide and spherical zirconium oxide to spherical alumina and sintering at normal pressure and isostatic pressing. However, the alumina ceramic needs to add more molding agents during the molding process, and also needs to be sintered at normal pressure and isostatic pressing. There will be a large size shrinkage during the molding and preparation process. When used for processing and preparing ceramic splitters, grinding treatment is required. However, the hardness of the alumina ceramic is above 2000HV, and the density is also very high, which greatly increases the difficulty of grinding and the loss of the grinding wheel during the grinding process; in addition, the price of chromium oxide is relatively high, which also greatly increases the cost of the product. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a ceramic trimming knife for dry forming of electrical porcelain, which is prepared by a one-time firing process, has a low dimensional shrinkage rate, a regular appearance, a sharp blade, good wear resistance and bending strength, and a long service life; the present invention also provides a preparation method thereof.

[0006] The method for preparing a ceramic trimming knife for dry forming of electric porcelain of the present invention comprises the following steps: (1) Feed material preparation: After melting the binder, add the plasticizer and the surfactant, mix them evenly, and obtain an organic plasticizer; add the surface-modified ceramic powder and the sintering aid to the molten organic plasticizer, mix and knead, and obtain a feed material; (2) Injection molding: The feed material is injection molded to obtain a molded body; (3) Extraction dewaxing: The formed body is placed in a dewaxing agent at 45-85°C for extraction dewaxing for 5-10 hours to obtain a dewaxed body; (4) Drying and sintering: The dewaxed body is dried, kept at 1480-1620°C for 1-5 hours, and sintered to obtain a ceramic trimming knife.

[0007] In step (1), the feed composition is: 88-92wt.% of surface-modified ceramic powder, 5-8wt.% of organic plasticizer, and 0.5-5wt.% of sintering aid.

[0008] In step (1), the surface-modified ceramic powder is a ceramic powder modified by a surface modifier; the surface modification process of the ceramic powder is as follows: the ceramic powder is added to a high-speed mixer, stirred and mixed evenly, and then the surface modifier is added, and the stirring and mixing is continued for 0.5-1h, and then sieved through a 30-mesh sieve to obtain a surface-modified ceramic powder.

[0009] Preferably, the ceramic powder is composed of 75-90wt.% spherical α-alumina powder and 10-25wt.% yttrium-stabilized zirconia powder; among the spherical α-alumina powder, 40-50wt.% of the spherical α-alumina powder with a median particle size of 0.2≤<0.5μm, 30-50wt.% of the spherical α-alumina powder with a median particle size of 0.5≤<1.0μm, and 10-20% of the spherical α-alumina powder with a median particle size of 1.0≤<1.5μm.

[0010] More preferably, the purity of the spherical α-alumina powder is ≥99.9%. The yttrium-stabilized zirconia powder is 3Y zirconia powder, with a median particle size of 0.3-1.0 μm and a purity of ≥99.5%.

[0011] Preferably, the surface modifier is one or more of an aluminate coupling agent, an aluminum zirconium coupling agent, and a zirconate coupling agent; and the amount of the surface modifier is 0.5-5% of the mass of the ceramic powder.

[0012] In step (1), the organic plasticizer is composed of 80-85wt.% of a binder, 5-15wt.% of a plasticizer, and 5-10wt.% of a surfactant.

[0013] Preferably, the binder is one or more of paraffin wax, microcrystalline wax, polymethyl acrylate, polyoxymethylene, polyvinyl chloride, high-density polyethylene resin, ABS resin, and EVA resin.

[0014] Preferably, the plasticizer is one or more of glycerol, dioctyl phthalate (DOP), polyethylene glycol 6000, and polyethylene glycol 8000.

[0015] Preferably, the surfactant is one or more of beeswax, oleic acid, stearic acid, vegetable oil, and Tween 80.

[0016] The preparation method of the organic plasticizer is as follows: adding a binder into a stainless steel crucible for melting at a melting temperature of 180-200° C., adding a plasticizer and a surfactant after the binder is completely melted, and maintaining the temperature at 180-200° C. for not less than 30 minutes to obtain the organic plasticizer.

[0017] In step (1), the sintering aid is one or more of rare earth oxides, titanium oxide, magnesium oxide, calcium carbonate, strontium oxide, strontium carbonate, and chromium oxide.

[0018] In step (2), the molding pressure is 5-10 MPa and the molding temperature is 110-150°C.

[0019] In step (3), the dewaxing agent may be any commercially available dewaxing agent, the main component of which is an alkane compound.

[0020] In step (4), the drying temperature is 60-80° C. and the drying time is 4-10 h. The drying is preferably carried out in an oven.

[0021] In step (4), during sintering, the temperature is raised to 1480-1620°C at a heating rate of 0.8-5°C / min and the heat preservation time is 1-5h. Preferably, the sintering is carried out in a sintering furnace.

[0022] The present invention also provides a ceramic trimming knife prepared by the preparation method.

[0023] Compared with the prior art, the present invention has the following beneficial effects: (1) The raw materials of the present invention are spherical α-alumina powders of different particle sizes for particle grading, and the surface of the ceramic powder is modified by a surface modifier, which significantly increases the amount of ceramic powder added during the feeding preparation process and greatly reduces the amount of organic plasticizer added. The reduction in the amount of organic plasticizer can reduce the shrinkage rate of the green body during the molding and cooling process, thereby avoiding cracking of the green body and improving the molding qualification rate. At the same time, the reduction in the organic matter content in the green body can significantly shorten the degreasing time, thereby reducing the sintering shrinkage rate, and finally obtaining a high-performance ceramic trimming knife with low shrinkage, high precision and low deformation; (2) The present invention uses a surface modifier to modify the ceramic powder, forming an organic molecular layer on the surface of the powder, thereby enhancing the interfacial compatibility between the inorganic powder and the organic resin, improving the dispersibility of the powder in the organic binder, and significantly reducing the amount of organic plasticizer. At the same time, the surface modifier can be converted into alumina and zirconia after the green body is sintered, thereby improving the density of the sintered product; (3) The present invention adopts an extraction dewaxing method, and the main binder components in the green body are removed by extraction, which can greatly reduce the volatilization time of organic matter in the sintering process, and the extracted mixture can be reused after distillation, thereby reducing production costs; the present invention adopts injection molding and one-time sintering molding processes, and the prepared ceramic trimming knife has a regular appearance, a sharp blade and good wear resistance. DETAILED DESCRIPTION

[0024] The present invention is further described below with reference to the examples. The raw materials used in the examples, unless otherwise specified, are all commercially available conventional raw materials; the process methods used in the examples, unless otherwise specified, are all conventional methods in the art.

[0025] The purity of the spherical α-alumina powder used in the embodiment is ≥99.9%; the yttrium-stabilized zirconia powder used is 3Y zirconia powder, with a median particle size between 0.3-1.0 μm and a purity of ≥99.5%.

[0026] The dewaxing agent used in the embodiment is a 320 type environmentally friendly dewaxing agent produced by Shenzhen Yougongrong Company.

[0027] Example 1 A method for preparing a ceramic trimming knife for dry forming of electric porcelain comprises the following steps: (1) Feed preparation: In terms of mass percentage, 50% paraffin wax and 30% high-density polyethylene resin are added into a stainless steel crucible, and the temperature is maintained between 180-200° C. for melting. When the paraffin wax and the high-density polyethylene resin are completely melted, 15% dioctyl phthalate and 5% stearic acid are added, and the mixture is kept at 180-200° C. for not less than 30 minutes to obtain an organic plasticizer. In terms of mass percentage, the ceramic powder is composed of 75% of spherical α-alumina powder and 25% of yttrium-stabilized zirconia powder, wherein the spherical α-alumina powder with a median particle size of 0.2 ≤ <0.5 μm accounts for 50 wt.%, the spherical α-alumina powder with a median particle size of 0.5 ≤ <1.0 μm accounts for 40 wt.%, and the spherical α-alumina powder with a median particle size of 1.0 ≤ <1.5 μm accounts for 10 wt.%; the above ceramic powder is added into a high-speed mixer with a material-to-ball ratio of 1:2, stirred and mixed for 3 hours, and then a zirconate coupling agent accounting for 5% of the mass of the ceramic powder is added, and the stirring and mixing is continued for 1 hour, and then sieved with a 30-mesh sieve to obtain a surface-modified ceramic powder; In terms of mass percentage, 7% of an organic plasticizer is melted, and then 88% of a surface-modified ceramic powder and 5% of a sintering aid (magnesium oxide and calcium oxide in a mass ratio of 1:1) are added, mixed, and a feed material is obtained; (2) Injection molding: preheat the injection molding machine to 120°C, add the prepared feed material into the hopper of the injection molding machine for injection molding, and the molding pressure is 8 MPa to obtain a molded body; (3) Extraction dewaxing: The formed body is placed in a dewaxing agent at 60°C for extraction dewaxing for 8 hours to obtain a dewaxed body; (4) Drying and sintering: The dewaxed body is dried in an oven at 70°C for 8 h, then placed in a sintering furnace, heated to 600°C at a heating rate of 1°C / min, and then heated to 1550°C at a heating rate of 5°C / min, and kept at this temperature for 3 h to obtain a ceramic trimming knife.

[0028] Example 2 A method for preparing a ceramic trimming knife for dry forming of electric porcelain comprises the following steps: (1) Feed preparation: In terms of mass percentage, 50% microcrystalline wax and 35% polymethyl acrylate are added into a stainless steel crucible, and the temperature is maintained between 180-200° C. for melting. When the polymethyl acrylate is completely melted, 10% polyethylene glycol 6000 and 5% beeswax are added, and the mixture is kept at 180-200° C. for not less than 30 minutes to obtain an organic plasticizer. In terms of mass percentage, the ceramic powder is composed of 85% of spherical α-alumina powder and 15% of yttrium-stabilized zirconia powder, 40wt.% of spherical α-alumina powder with a median particle size of 0.2≤<0.5μm, 50wt.% of spherical α-alumina powder with a median particle size of 0.5≤<1.0μm, and 10wt.% of spherical α-alumina powder with a median particle size of 1.0≤<1.5μm; the above ceramic powder is added into a high-speed mixer with a material-to-ball ratio of 1:1, stirred and mixed for 2h, and then an aluminum-zirconium coupling agent accounting for 3% of the mass of the ceramic powder is added, and the stirring and mixing is continued for 1h, and then sieved with a 30-mesh sieve to obtain a surface-modified ceramic powder; In terms of mass percentage, 8% of an organic plasticizer is melted, and then 91.5% of a surface-modified ceramic powder and 0.5% of a sintering aid (calcium carbonate and strontium carbonate in a mass ratio of 1:1) are added, mixed, and a feed material is obtained; (2) Injection molding: preheat the injection molding machine to 150°C, add the prepared feed material into the hopper of the injection molding machine for injection molding, and the molding pressure is 5 MPa to obtain a molded body; (3) Extraction dewaxing: The formed body is placed in a dewaxing agent at 45°C for extraction dewaxing for 10 hours to obtain a dewaxed body; (4) Drying and sintering: The dewaxed body is dried in an oven at 80°C for 4 h, then placed in a sintering furnace, heated to 580°C at a heating rate of 1.5°C / min, and then heated to 1480°C at a heating rate of 5°C / min. The temperature is kept at this temperature for 5 h and sintered to obtain a ceramic trimming knife.

[0029] Example 3 A method for preparing a ceramic trimming knife for dry forming of electric porcelain comprises the following steps: (1) Feed preparation: In terms of mass percentage, 50% paraffin wax, 20% high-density polyethylene resin, and 15% ABS resin are added into a stainless steel crucible, and the temperature is maintained between 180-200° C. for melting. When the high-density polyethylene resin is completely melted, 5% propylene glycol, 5% stearic acid, and 5% beeswax are added, and the mixture is kept at 180-200° C. for not less than 30 minutes to obtain an organic plasticizer. In terms of mass percentage, the ceramic powder is composed of 90% spherical α-alumina powder and 10% yttrium-stabilized zirconia powder, wherein the spherical α-alumina powder with a median particle size of 0.2 ≤ <0.5 μm accounts for 50 wt.%, the spherical α-alumina powder with a median particle size of 0.5 ≤ <1.0 μm accounts for 30 wt.%, and the spherical α-alumina powder with a median particle size of 1.0 ≤ <1.5 μm accounts for 20 wt.%; the above ceramic powder is added into a high-speed mixer with a material-to-ball ratio of 1:2, and after stirring and mixing for 4 hours, an aluminate coupling agent accounting for 1% of the mass of the ceramic powder is added, and stirring and mixing is continued for 0.5 hours, and then sifted with a 30-mesh sieve to obtain a surface-modified ceramic powder; In terms of mass percentage, 5% of an organic plasticizer is melted, and then 92% of a surface-modified ceramic powder and 3% of a sintering aid (chromium oxide, strontium oxide and lanthanum oxide in a mass ratio of 1:1:1) are added, and mixed to obtain a feed material; (2) Injection molding: preheat the injection molding machine to 110°C, add the prepared feed material into the hopper of the injection molding machine for injection molding, and the molding pressure is 10 MPa to obtain a molded body; (3) Extraction dewaxing: The formed body is placed in a dewaxing agent at 85°C for extraction dewaxing for 5 hours to obtain a dewaxed body; (4) Drying and sintering: The dewaxed body is dried in an oven at 60°C for 10 h, then placed in a sintering furnace, heated to 620°C at a heating rate of 0.8°C / min, and then heated to 1620°C at a heating rate of 5°C / min, and kept at this temperature for 1 h to obtain a ceramic trimming knife.

[0030] Comparative Example 1 The only difference between this comparative example and Example 1 is that all spherical α alumina powders are spherical α alumina powders with a median particle size of 0.5≤<1.0μm; in addition, in order to achieve an injection molding effect close to that of Example 1, the feed composition of this comparative example is: 12.5wt.% of organic plasticizer, 82.5wt.% of surface-modified ceramic powder, and 5wt.% of sintering aid.

[0031] Comparative Example 2 The only difference between this comparative example and Example 1 is that all spherical α alumina powders are spherical α alumina powders with a median particle size of 0.2≤<0.5μm; in addition, in order to achieve an injection molding effect close to that of Example 1, the feed composition of this comparative example is: 15wt.% of organic plasticizer, 80wt.% of surface-modified ceramic powder, and 5wt.% of sintering aid.

[0032] Comparative Example 3 The only difference between this comparative example and Example 1 is that ceramic powder without surface modification treatment is used; in addition, in order to achieve an injection molding effect close to that of Example 1, the feed composition of this comparative example is: 14wt.% of organic plasticizer, 81wt.% of ceramic powder, and 5wt.% of sintering aid.

[0033] Comparative Example 4 The difference between this comparative example and Example 1 is that thermal degreasing is used instead of extractive dewaxing. The thermal degreasing process is as follows: the formed body is placed in a degreasing furnace, heated to 100°C, kept warm for 30 minutes, heated to 230°C, kept warm for 450 minutes, heated to 650°C, kept warm for 350 minutes, and cooled to room temperature with the furnace.

[0034] Comparative Example 5 The only difference between this comparative example and Example 1 is that no sintering aid is added, and the sintering aid is replaced by an equal mass of surface-modified ceramic powder.

[0035] The ceramic trimming knives prepared in each embodiment and comparative example were subjected to performance tests, and the test methods were as follows: the density of the product was tested by the Archimedes drainage method; the bending strength of the product was tested by the three-point bending method; the Vickers hardness of the sample was tested by a Vickers hardness tester; the product size was measured by a vernier caliper and the size shrinkage rate was calculated, where the size shrinkage rate = (size before sintering - size after sintering) / size before sintering × 100%; the service life was calculated by the number of pieces of the same ceramic piece that could be processed by a single ceramic trimming knife. The test results are shown in Table 1.

[0036] As can be seen from Table 1, the ceramic trimming knives prepared in Examples 1-3 of the present invention have low size shrinkage, high density, high bending strength and hardness, and long service life. Comparative Example 1 uses all spherical α-alumina powders with larger particle sizes, and Comparative Example 2 uses all spherical α-alumina powders with smaller particle sizes. In order to achieve an injection molding effect close to that of Example 1, it is necessary to increase the amount of organic plasticizer added accordingly, and the size shrinkage of the ceramic trimming knife is significantly increased, and the bending strength, fracture toughness and hardness are also reduced. Comparative Example 3 uses ceramic powders that have not been surface-modified. In order to achieve an injection molding effect close to that of Example 1, it is also necessary to increase the amount of organic plasticizer added accordingly. At the same time, the size shrinkage of the ceramic trimming knife is significantly increased, and the bending strength, fracture toughness and hardness indicators are significantly reduced. Comparative Example 4 uses thermal degreasing instead of extractive dewaxing, and the degreasing time is increased. The product is easily cracked and deformed during the thermal degreasing process, and the mechanical properties of the ceramic trimming knife obtained are reduced, the regularity and sharpness are reduced, and the service life is shortened. In Comparative Example 5, no sintering aid is added, the density of the product is significantly reduced, the mechanical indicators such as bending strength, fracture toughness and hardness are significantly reduced, and the service life is short.

Claims

1. A method for preparing a ceramic trimming knife for dry forming of electric porcelain, characterized in that: The following steps are involved: (1) Feed material preparation: After melting the binder, add the plasticizer and the surfactant, mix them evenly, and obtain an organic plasticizer; add the surface-modified ceramic powder and the sintering aid to the molten organic plasticizer, mix and knead, and obtain a feed material; (2) Injection molding: The feed material is injection molded to obtain a molded body; (3) Extraction dewaxing: The formed body is placed in a dewaxing agent at 45-85°C for extraction dewaxing for 5-10 hours to obtain a dewaxed body; (4) Drying and sintering: drying the dewaxed body, keeping it at 1480-1620°C for 1-5h, and sintering it to obtain a ceramic trimming knife; In step (1), the feed composition is: 88-92wt.% of surface-modified ceramic powder, 5-8wt.% of organic plasticizer, and 0.5-5wt.% of sintering aid; The surface-modified ceramic powder is a ceramic powder modified by a surface modifier; The ceramic powder is composed of 75-90wt.% of spherical α-alumina powder and 10-25wt.% of yttrium-stabilized zirconia powder; among the spherical α-alumina powder, 40-50wt.% of spherical α-alumina powder with a median particle size of 0.2≤<0.5μm, 30-50wt.% of spherical α-alumina powder with a median particle size of 0.5≤<1.0μm, and 10-20% of spherical α-alumina powder with a median particle size of 1.0≤<1.5μm.

2. The method for preparing a ceramic trimming knife for dry forming of electrical porcelain according to claim 1, characterized in that: In step (1), the surface modification process of the ceramic powder is as follows: the ceramic powder is added to a high-speed mixer, and after stirring and mixing evenly, a surface modifier is added, and stirring and mixing is continued for 0.5-1h, and then sieved through a 30-mesh sieve to obtain a surface-modified ceramic powder.

3. The method for preparing a ceramic trimming knife for dry forming of electrical porcelain according to claim 1, characterized in that: The purity of spherical α-alumina powder is ≥99.9%. Yttrium-stabilized zirconia powder is 3Y zirconia powder with a median particle size of 0.3-1.0μm and a purity of ≥99.5%.

4. The method for preparing a ceramic trimming knife for dry forming of electrical porcelain according to claim 1, characterized in that: The surface modifier is one or more of an aluminate coupling agent, an aluminum zirconium coupling agent, and a zirconate coupling agent; the amount of the surface modifier is 0.5-5% of the mass of the ceramic powder.

5. The method for preparing a ceramic trimming knife for dry forming of electrical porcelain according to claim 1, characterized in that: In step (1), the organic plasticizer is composed of 80-85wt.% of a binder, 5-15wt.% of a plasticizer, and 5-10wt.% of a surfactant.

6. The method for preparing a ceramic trimming knife for dry forming of electrical porcelain according to claim 1, characterized in that: The binder is one or more of paraffin wax, microcrystalline wax, polymethyl acrylate, polyoxymethylene, polyvinyl chloride, high-density polyethylene resin, ABS resin, and EVA resin; The plasticizer is one or more of glycerol, dioctyl phthalate, polyethylene glycol 6000, and polyethylene glycol 8000; The surfactant is one or more of beeswax, oleic acid, stearic acid, vegetable oil and Tween 80.

7. The method for preparing a ceramic trimming knife for dry forming of electrical porcelain according to claim 1, characterized in that: In step (1), the sintering aid is one or more of rare earth oxides, titanium oxide, magnesium oxide, calcium carbonate, strontium oxide, strontium carbonate, and chromium oxide.

8. The method for preparing a ceramic trimming knife for dry forming of electrical porcelain according to claim 1, characterized in that: In step (2), the molding pressure is 5-10 MPa and the molding temperature is 110-150°C.

9. The method for preparing a ceramic trimming knife for dry forming of electrical porcelain according to claim 1, characterized in that: In step (4), the drying temperature is 60-80°C and the drying time is 4-10h; During sintering, the temperature is raised to 1480-1620° C. at a heating rate of 0.8-5° C. / min and the heat preservation time is 1-5 hours. Sintering is preferably carried out in a sintering furnace.

10. A ceramic trimming knife for dry forming of electric porcelain, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Alumina ceramic, preparation method thereof and ceramic chopper

    CN109485393A

  • Ceramic chopper and preparation method thereof

    CN115784754A

  • Method for producing transparent ceramic component by injection molding

    CN105693255A

  • Preparation method for transparent aluminum oxide ceramics

    CN106966709A

  • Sintered alumina ceramic, method for producing the same, and cutting tool

    US20030027707A1

Cited By

  • High-uniformity yttria-stabilized zirconia feed for optical fiber sleeve as well as preparation method and application of high-uniformity yttria-stabilized zirconia feed

    CN122586552A