Ceramic and preparation method and application thereof

By regulating the amount and particle size of the ion substitution in the ceramic and combining the resin composition, ceramic circuit substrates are prepared, which solves the problem of taking into account both thermal conductivity and dielectric loss in ceramics, and a circuit substrate with low dielectric loss and high thermal conductivity is achieved.

CN118955107AActive Publication Date: 2024-11-15ZHEJIANG WAZAM NEW MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411442151.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-15
Estimated Expiration
2044-10-16

AI Technical Summary

Technical Problem

The existing ceramics cannot take into account low dielectric loss while improving thermal conductivity, and the high filling amount makes the circuit substrate prepared unable to have both low dielectric loss and high thermal conductivity.

Method used

By regulating the relationship between the amount of ion substitution and particle size in ceramics, improving grain size and density, optimizing microstructure, and reducing interface effects, preparing ceramics with the chemical formula Mg2-xGaxSi1-xO4, combining resin compositions, and preparing circuit substrates to achieve Low dielectric loss and high thermal conductivity.

Benefits of technology

The low dielectric loss and high thermal conductivity of ceramics are achieved, and an effective thermal conductivity path is constructed to improve the thermal conductivity of the circuit substrate, while reducing dielectric loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to ceramic and a preparation method and application thereof, the chemical formula of the ceramic is Mg2-xGaxSi1-xAlxO4, x is ion substitution amount, x is more than 0 and less than or equal to 0.05, and when x is more than 0 and less than or equal to 0.04, the particle size of the ceramic is (10 + 1000x) [mu] m to (15 + 1000x) [mu] m, and when x is more than 0.04 and less than or equal to 0.05, the particle size of the ceramic is 50 [mu] m to 55 [mu] m. According to the present invention, the relationship between the ion substitution amount x and the particle size in the ceramic is regulated so as to make the ceramic simultaneously have low dielectric loss and high thermal conductivity, such that the circuit substrate prepared from the ceramic can simultaneously have low dielectric loss and high thermal conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramics, and in particular to ceramics and a preparation method and application thereof. Background Art

[0002] When existing ceramics have high thermal conductivity, their dielectric loss is also high, which cannot meet the use requirements of high-frequency circuit substrates; when ceramics have low dielectric loss, their thermal conductivity is also low, and it is necessary to increase the filling amount of ceramics to improve the thermal conductivity of the circuit substrate. However, too high a filling amount of ceramics will cause the prepared circuit substrate to be unable to take into account both low dielectric loss and high thermal conductivity. Summary of the invention

[0003] Based on this, it is necessary to provide a ceramic and a preparation method and application thereof to address the above problems. The ceramic can have both low dielectric loss and high thermal conductivity, and the circuit substrate prepared using the ceramic can have both low dielectric loss and high thermal conductivity.

[0004] The present invention provides a ceramic, wherein the chemical formula of the ceramic is Mg 2-x Ga x Si 1-x Al x O4, wherein x is the amount of ion substitution, 0<x≤0.05, and when 0<x≤0.04, the particle size of the ceramic is (10+1000x)μm to (15+1000x)μm, and when 0.04<x≤0.05, the particle size of the ceramic is 50μm to 55μm.

[0005] In one of the embodiments, the mass fraction of the MgSiO3 impurity phase in the ceramic is less than or equal to 1%.

[0006] In one embodiment, x>0.02.

[0007] The present invention provides a method for preparing ceramics, comprising the following steps: MgO, Ga2O3, Al2O3 and SiO2 are mixed as raw materials, wherein the molar ratio of Mg, Ga, Si and Al in the raw materials is 2-x:x:1-x:x, and 0<x≤0.05; The raw material is subjected to a first ball milling to obtain a first ball milled powder; Drying, grinding, sieving and pre-calcining the powder after the first ball milling to obtain a pre-calcined powder; Grinding and sieving the pre-sintered powder again, and ball milling the powder for a second time to obtain a second ball milled powder; The powder after the second ball milling is dried, and subjected to the first screening, granulation, the second screening, sintering, crushing and screening to obtain the ceramic.

[0008] In one embodiment, the method for preparing the ceramic satisfies at least one of the following conditions: (1) The purity of the raw materials is above 99.5% and the particle size is below 20 μm; (2) The first ball milling uses ball milling beads with a particle size of 2 mm to 5 mm, and the solvent used includes at least one of deionized water or ethanol; (3) The second ball milling uses ball milling beads with a particle size of 2 mm-5 mm, and the solvent used includes at least one of deionized water or ethanol.

[0009] The invention also provides a resin composition, comprising a resin and the ceramic.

[0010] In one embodiment, the resin composition satisfies at least one of the following conditions: (1) The resin includes at least one of fluorine-containing resin, epoxy resin, hydrocarbon resin or polyphenylene ether resin; (2) The mass of the ceramic is 30%-70% of the total mass of the resin and the ceramic.

[0011] The invention also provides a prepreg made from the resin composition.

[0012] The invention also provides a circuit substrate made of the prepreg.

[0013] The invention also provides a printed circuit board made of the circuit substrate.

[0014] The present invention improves the grain size and density of the ceramic by regulating the relationship between the amount of ion substitution and the particle size in the ceramic, thereby improving the uniformity of the ceramic microstructure and optimizing the grain boundary structure of the ceramic, while reducing the interface effect between ceramic particles, reducing scattering and polarization losses, and making the ceramic have both low dielectric loss and high thermal conductivity.

[0015] Therefore, when the ceramic of the present invention is applied to a circuit substrate, a more effective heat conduction path can be constructed, and the thermal conductivity of the circuit substrate can be improved, so that the circuit substrate can have both low dielectric loss and high thermal conductivity. DETAILED DESCRIPTION

[0016] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0017] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.

[0018] The chemical formula of the ceramic provided by the present invention is Mg 2-x Ga x Si 1-x Al x O4, wherein x is the amount of ion substitution, 0<x≤0.05, and when 0<x≤0.04, the particle size of the ceramic is (10+1000x)μm to (15+1000x)μm, and when 0.04<x≤0.05, the particle size of the ceramic is 50μm to 55μm.

[0019] For example, when the ion substitution amount x is 0.01, the particle size of the ceramic is 20μm-25μm, and more preferably 20μm-22μm. When the ion substitution amount x is 0.02, the particle size of the ceramic is 30μm-35μm, and more preferably 30μm-32μm. When the ion substitution amount x is 0.03, the particle size of the ceramic is 40μm-45μm, and more preferably 40μm-42μm. When the ion substitution amount x is 0.04, the particle size of the ceramic is 50μm-55μm, and more preferably 50μm-52μm.

[0020] Optionally, the mass fraction of the MgSiO3 impurity phase in the ceramic of the present invention is less than or equal to 1%. This can reduce the formation of conductive channels with the impurity phase as the medium, reduce the influence of impurities on the crystal structure of the ceramic, help form a regular and orderly crystal structure, improve the uniformity and density of the ceramic, reduce the formation of defects, thereby improving thermal conductivity and reducing dielectric loss.

[0021] The thermal conductivity and dielectric loss of the ceramic of the present invention are related to the ion substitution amount x and the particle size. For example, as the ion substitution amount x increases, the dielectric loss of the ceramic will decrease, and as the ion substitution amount x increases, the optimal particle size will also increase accordingly. As the particle size increases, the thermal conductivity of the ceramic increases, but the dielectric loss also increases.

[0022] Optionally, the preferred ion substitution amount x>0.02, within this range, the thermal conductivity and dielectric loss of the ceramic are relatively better, which is conducive to the preparation of circuit substrates with excellent thermal conductivity and dielectric loss. Furthermore, when the ion substitution amount is within this range, the thermal conductivity of the ceramic can be improved and the dielectric loss of the ceramic can be reduced by further reducing the content of the MgSiO3 impurity phase.

[0023] The present invention has different ion substitution amounts in the ceramic, and different grain sizes and densities of the ceramic. The present invention improves the grain size and density of the ceramic by regulating the relationship between the ion substitution amount x and the particle size in the ceramic, thereby improving the uniformity of the ceramic microstructure, optimizing the grain boundary structure of the ceramic, and reducing the interface effect between the ceramic particles, reducing the scattering and polarization losses, so that the ceramic has both low dielectric loss and high thermal conductivity. Specifically, the dielectric loss of the ceramic can be as low as 0.5×10 -4 , the thermal conductivity can be as high as 13W / mk.

[0024] The present invention is not particularly limited to the method for preparing the ceramic. As a specific example, the method for preparing the ceramic includes the following steps: MgO, Ga2O3, Al2O3 and SiO2 are mixed as raw materials, wherein the molar ratio of Mg, Ga, Si and Al is 2-x:x:1-x:x, and 0<x≤0.05; wherein the purity of the raw materials is preferably above 99.5%, more preferably above 99.99%, and the particle size of the raw materials is preferably below 20 μm, thereby, the generation of impurities can be reduced by selecting the purity and particle size of the raw materials, which is beneficial to improving the thermal conductivity of the ceramic and reducing the dielectric loss of the ceramic.

[0025] Then the raw materials are ball-milled for the first time; among them, ball milling beads with a particle size of 2mm-5mm are preferred, such as ZrO2 ball milling beads, quartz ball milling beads, alumina ball milling beads, etc., and ZrO2 ball milling beads with a particle size of 2mm-3mm are further preferred. The ball milling speed is preferably 150r / min-250r / min, and the ball milling time is 20h-36h, which can make the raw materials mixed more evenly and help reduce the generation of impurities. In addition, the solvent during ball milling is not limited, and is preferably deionized water, ethanol, etc.

[0026] The powder after the first ball milling is then dried, ground, sieved and pre-calcined, wherein the drying temperature is preferably 70°C-90°C, the time is preferably 20h-36h, after grinding, it is preferably sieved through a 120-mesh standard sieve, the pre-calcining temperature is preferably 1100°C-1200°C, and the time is preferably 3h-5h.

[0027] The pre-calcined powder is then ground and sieved again, and ball milled for the second time; wherein, ball milling beads with a particle size of 2mm-5mm are preferred during ball milling, such as ZrO2 ball milling beads, quartz ball milling beads, alumina ball milling beads, etc., and ZrO2 ball milling beads with a particle size of 2mm-3mm are further preferred, which can make the raw materials mixed more evenly and help reduce the generation of impurities. The solvent used in ball milling is not limited, and is preferably deionized water, ethanol, etc. In addition, a 120-mesh standard sieve is preferably used for sieving.

[0028] The powder after the second ball milling is then dried, and subjected to the first screening, granulation, second screening, sintering, crushing and screening to obtain the ceramic, wherein the drying temperature is preferably 70°C-90°C, the time is preferably 20h-36h, the first screening is preferably a 200-mesh standard sieve, the granulation is preferably carried out in a PVA solution, the second screening is preferably an 80-mesh standard sieve, the sintering temperature is preferably 1300°C-1500°C, and the time is preferably 2h-4h.

[0029] By adopting the preparation method provided by the present invention, ceramics having a satisfactory relationship between the ion substitution amount x and the particle size can be prepared. In addition, the generation of impurities in the ceramics can be reduced, so that the prepared ceramics can have both low dielectric loss and high thermal conductivity.

[0030] The present invention also provides a resin composition for preparing a circuit substrate, wherein the resin composition comprises a resin and the ceramic.

[0031] The present invention does not impose any special limitation on the selection of resin in the resin composition, including but not limited to fluorine-containing resin, epoxy resin, hydrocarbon resin or polyphenylene ether resin, etc., and is further preferably a fluorine-containing resin, wherein the fluorine-containing resin includes but is not limited to at least one of polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene copolymer (ETFE) or ethylene-chlorotrifluoroethylene copolymer (ECTFE), and more preferably polytetrafluoroethylene (PTFE) with low dielectric loss, so that the obtained circuit substrate has better dielectric properties.

[0032] Optionally, the mass of the ceramic is 30%-70% of the total mass of the resin and the ceramic. Considering that the agglomeration problem of the ceramic will increase the dielectric loss, further, the mass of the ceramic is preferably 50%-70% of the total mass of the resin and the ceramic, and more preferably 55%-65%, so that the circuit substrate can have higher thermal conductivity and lower dielectric loss.

[0033] Optionally, the ceramic is treated with a silane coupling agent, which is beneficial to improve the dispersibility of the ceramic in the resin composition, and further beneficial to improve the dielectric loss performance and thermal conductivity of the circuit substrate. The silane coupling agent is preferably at least one of a fluorine-containing silane coupling agent or an aminosilane coupling agent, and more preferably at least one of KH550, Z6124, and F8261.

[0034] The present invention also provides a prepreg made of the resin composition. The present invention does not limit the specific preparation method of the prepreg from the resin composition. Specifically, the resin composition is impregnated or coated on a reinforcing material, and dried at 120° C.-180° C. for 1.5 min-6 min to obtain an impregnated prepreg or a coated prepreg. Preferably, the reinforcing material is selected from at least one of glass fiber cloth, aramid cloth, PET film or carbon fiber cloth. The coated prepreg can choose whether to peel off the reinforcing material according to actual use requirements.

[0035] The present invention also provides a circuit substrate made of the prepreg, comprising a dielectric layer and a conductive layer arranged on at least one surface of the dielectric layer, wherein the dielectric layer is pressed from one or at least two superimposed prepregs as described above, and the conductive layer is a metal foil layer, preferably a copper foil. Since the ceramic of the present invention can have both low dielectric loss and high thermal conductivity, the circuit substrate prepared using the ceramic of the present invention can have both low dielectric loss and high thermal conductivity.

[0036] The present invention also provides a printed circuit board made of the circuit substrate, wherein the printed circuit board is mainly made of the circuit substrate through processes such as developing, etching, drilling, degumming, copper deposition, electroplating and pressing.

[0037] Hereinafter, the ceramic and its preparation method and application will be further described through the following specific examples.

[0038] Example 1 MgO, Ga2O3, Al2O3 and SiO2 with a purity of 99.99% and a particle size of 5μm are used as raw materials, prepared in a molar ratio of Mg:Ga:Si:Al of 1.99:0.01:0.99:0.01 and placed in a ball mill filled with ZrO2 ball milling beads with a diameter of 3mm. Deionized water is added to the ball mill for the first low-speed ball milling at a speed of 170r / min and a ball milling time of 24h.

[0039] The powder after the first ball milling was dried in a forced air oven at 80°C for 24 h, then ground in a mortar, passed through a 120-mesh standard sieve, and then pre-calcined at 1200°C for 4 h.

[0040] The pre-sintered powder was ground, passed through a 200-mesh standard sieve, and put into the ball mill again. ZrO2 ball milling beads with a diameter of 3 mm and deionized water were added for the second ball milling. The ball milling speed was 300 r / min and the ball milling time was 12 h.

[0041] The powder after the second ball milling was dried at 80°C for 24h, passed through a 200-mesh standard sieve, put into a granulator for granulation (1% PVA solution by mass), passed through an 80-mesh standard sieve, and finally sintered at 1450°C for 3h. After crushing, the powder was screened to obtain a granule with the chemical formula of Mg 1.99 Ga 0.01 Si 0.99 Al 0.01 O4, ceramics with a particle size of 20μm-25μm, and the mass fraction of MgSiO3 impurity phase in the ceramics is 0.5%.

[0042] Example 2 MgO, Ga2O3, Al2O3 and SiO2 with a purity of 99.99% and a particle size of 5 μm are used as raw materials, prepared in a molar ratio of Mg:Ga:Si:Al of 1.98:0.02:0.98:0.02 and placed in a ball mill filled with ZrO2 ball milling beads with a diameter of 3 mm. Deionized water is added to the ball mill for the first low-speed ball milling at a speed of 170 r / min for 24 h.

[0043] The powder after the first ball milling was dried in a forced air oven at 80°C for 24 h, then ground in a mortar, passed through a 120-mesh standard sieve, and then pre-calcined at 1200°C for 4 h.

[0044] The pre-sintered powder was ground, passed through a 200-mesh standard sieve, and put into the ball mill again. ZrO2 ball milling beads with a diameter of 3 mm and deionized water were added for the second ball milling. The ball milling speed was 300 r / min and the ball milling time was 12 h.

[0045] The powder after the second ball milling was dried at 80°C for 24h, passed through a 200-mesh standard sieve, put into a granulator for granulation (1% PVA solution by mass), passed through an 80-mesh standard sieve, and finally sintered at 1450°C for 3h. After crushing, the powder was screened to obtain a granule with the chemical formula of Mg 1.98 Ga 0.02 Si 0.98 Al 0.02 O4, ceramics with a particle size of 30μm-35μm, and the mass fraction of MgSiO3 impurity phase in the ceramics is 0.4%.

[0046] Example 3 MgO, Ga2O3, Al2O3 and SiO2 with a purity of 99.99% and a particle size of 5 μm are used as raw materials, prepared in a molar ratio of Mg:Ga:Si:Al of 1.97:0.03:0.97:0.03 and placed in a ball mill filled with ZrO2 ball milling beads with a diameter of 3 mm. Deionized water is added to the ball mill for the first low-speed ball milling at a speed of 170 r / min and a ball milling time of 24 h.

[0047] The powder after the first ball milling was dried in a forced air oven at 80°C for 24 h, then ground in a mortar, passed through a 120-mesh standard sieve, and then pre-calcined at 1200°C for 4 h.

[0048] The pre-sintered powder was ground, passed through a 200-mesh standard sieve, and put into the ball mill again. ZrO2 ball milling beads with a diameter of 3 mm and deionized water were added for the second ball milling. The ball milling speed was 300 r / min and the ball milling time was 12 h.

[0049] The powder after the second ball milling was dried at 80°C for 24h, passed through a 200-mesh standard sieve, put into a granulator for granulation (1% PVA solution by mass), passed through an 80-mesh standard sieve, and finally sintered at 1450°C for 3h. After crushing, the powder was screened to obtain a granule with the chemical formula of Mg 1.97 Ga 0.03 Si 0.97 Al 0.03 O4, ceramics with a particle size of 40μm-45μm, and the mass fraction of MgSiO3 impurity phase in the ceramics is 0.3%.

[0050] Example 4 MgO, Ga2O3, Al2O3 and SiO2 with a purity of 99.99% and a particle size of 5 μm are used as raw materials, prepared in a molar ratio of Mg:Ga:Si:Al of 1.96:0.04:0.96:0.04 and placed in a ball mill filled with ZrO2 ball milling beads with a diameter of 3 mm. Deionized water is added to the ball mill for the first low-speed ball milling at a speed of 170 r / min and a ball milling time of 24 h.

[0051] The powder after the first ball milling was dried in a forced air oven at 80°C for 24 h, then ground in a mortar, passed through a 120-mesh standard sieve, and then pre-calcined at 1200°C for 4 h.

[0052] The pre-sintered powder was ground, passed through a 200-mesh standard sieve, and put into the ball mill again. ZrO2 ball milling beads with a diameter of 3 mm and deionized water were added for the second ball milling. The ball milling speed was 300 r / min and the ball milling time was 12 h.

[0053] The powder after the second ball milling was dried at 80°C for 24h, passed through a 200-mesh standard sieve, put into a granulator for granulation (1% PVA solution by mass), passed through an 80-mesh standard sieve, and finally sintered at 1450°C for 3h. After crushing, the powder was screened to obtain a granule with the chemical formula of Mg 1.96 Ga 0.04 Si 0.96 Al 0.04 O4, ceramics with a particle size of 50μm-55μm, and the mass fraction of MgSiO3 impurity phase in the ceramics is 0.3%.

[0054] Example 5 MgO, Ga2O3, Al2O3 and SiO2 with a purity of 99.99% and a particle size of 5 μm are used as raw materials, prepared in a molar ratio of Mg:Ga:Si:Al of 1.95:0.05:0.95:0.05 and placed in a ball mill filled with ZrO2 ball milling beads with a diameter of 3 mm. Deionized water is added to the ball mill for the first low-speed ball milling at a speed of 170 r / min for 24 h.

[0055] The powder after the first ball milling was dried in a forced air oven at 80°C for 24 h, then ground in a mortar, passed through a 120-mesh standard sieve, and then pre-calcined at 1200°C for 4 h.

[0056] The pre-sintered powder was ground, passed through a 200-mesh standard sieve, and put into the ball mill again. ZrO2 ball milling beads with a diameter of 3 mm and deionized water were added for the second ball milling. The ball milling speed was 300 r / min and the ball milling time was 12 h.

[0057] The powder after the second ball milling was dried at 80°C for 24h, passed through a 200-mesh standard sieve, put into a granulator for granulation (1% PVA solution by mass), passed through an 80-mesh standard sieve, and finally sintered at 1450°C for 3h. After crushing, the powder was screened to obtain a granule with the chemical formula of Mg 1.95 Ga 0.05 Si 0.95 Al 0.05 O4, ceramics with a particle size of 50μm-55μm, and the mass fraction of MgSiO3 impurity phase in the ceramics is 0.1%.

[0058] Example 6 MgO, Ga2O3, Al2O3 and SiO2 with a purity of 99.99% and a particle size of 5 μm are used as raw materials, prepared in a molar ratio of Mg:Ga:Si:Al of 1.985:0.015:0.985:0.015 and placed in a ball mill filled with ZrO2 ball milling beads with a diameter of 3 mm. Deionized water is added to the ball mill for the first low-speed ball milling at a speed of 170 r / min and a ball milling time of 24 h.

[0059] The powder after the first ball milling was dried in a forced air oven at 80°C for 24 h, then ground in a mortar, passed through a 120-mesh standard sieve, and then pre-calcined at 1200°C for 4 h.

[0060] The pre-sintered powder was ground, passed through a 200-mesh standard sieve, and put into the ball mill again. ZrO2 ball milling beads with a diameter of 3 mm and deionized water were added for the second ball milling. The ball milling speed was 300 r / min and the ball milling time was 12 h.

[0061] The powder after the second ball milling was dried at 80°C for 24h, passed through a 200-mesh standard sieve, put into a granulator for granulation (1% PVA solution by mass), passed through an 80-mesh standard sieve, and finally sintered at 1450°C for 3h. After crushing, the powder was screened to obtain a granule with the chemical formula of Mg 1.985 Ga 0.015 Si 0.985 Al 0.015 O4, ceramics with a particle size of 25μm-30μm, and the mass fraction of MgSiO3 impurity phase in the ceramics is 0.4%.

[0062] Example 7 MgO, Ga2O3, Al2O3 and SiO2 with a purity of 99.99% and a particle size of 5 μm are used as raw materials, prepared in a molar ratio of Mg:Ga:Si:Al of 1.955:0.045:0.955:0.045 and placed in a ball mill filled with ZrO2 ball milling beads with a diameter of 3 mm. Deionized water is added to the ball mill for the first low-speed ball milling at a speed of 170 r / min for 24 h.

[0063] The powder after the first ball milling was dried in a forced air oven at 80°C for 24 h, then ground in a mortar, passed through a 120-mesh standard sieve, and then pre-calcined at 1200°C for 4 h.

[0064] The pre-sintered powder was ground, passed through a 200-mesh standard sieve, and put into the ball mill again. ZrO2 ball milling beads with a diameter of 3 mm and deionized water were added for the second ball milling. The ball milling speed was 300 r / min and the ball milling time was 12 h.

[0065] The powder after the second ball milling was dried at 80°C for 24h, passed through a 200-mesh standard sieve, put into a granulator for granulation (1% PVA solution by mass), passed through an 80-mesh standard sieve, and finally sintered at 1450°C for 3h. After crushing, the powder was screened to obtain a granule with the chemical formula of Mg 1.955 Ga 0.045 Si 0.955 Al 0.045 O4, ceramics with a particle size of 50μm-55μm, and the mass fraction of MgSiO3 impurity phase in the ceramics is 0.1%.

[0066] Example 8 MgO, Ga2O3, Al2O3 and SiO2 with a purity of 99% and a particle size of 21μm are used as raw materials, prepared in a molar ratio of Mg:Ga:Si:Al of 1.99:0.01:0.99:0.01 and placed in a ball mill filled with ZrO2 ball milling beads with a diameter of 3mm. Deionized water is added to the ball mill for the first low-speed ball milling. The ball milling speed is 170r / min and the ball milling time is 24h.

[0067] The powder after the first ball milling was dried in a forced air oven at 80 °C for 24 h, then ground in a mortar, passed through a 120-mesh standard sieve, and then pre-calcined at 1100 °C for 5 h.

[0068] The pre-sintered powder was ground, passed through a 200-mesh standard sieve, and put into the ball mill again. ZrO2 ball milling beads with a diameter of 3 mm and deionized water were added for the second ball milling. The ball milling speed was 300 r / min and the ball milling time was 12 h.

[0069] The powder after the second ball milling was dried at 80°C for 24h, passed through a 200-mesh standard sieve, put into a granulator for granulation (1% PVA solution by mass), passed through an 80-mesh standard sieve, and finally sintered at 1400°C for 3h. After crushing, the powder was screened to obtain a 1% PVA solution with the chemical formula of Mg 1.99 Ga 0.01 Si 0.99 Al 0.01 O4, ceramics with a particle size of 20μm-25μm, and the mass fraction of MgSiO3 impurity phase in the ceramics is 1.5%.

[0070] Comparative Example 1 MgO, Ga2O3, Al2O3 and SiO2 with a purity of 99.99% and a particle size of 5μm are used as raw materials, prepared in a molar ratio of Mg:Ga:Si:Al of 1.99:0.01:0.99:0.01 and placed in a ball mill filled with ZrO2 ball milling beads with a diameter of 3mm. Deionized water is added to the ball mill for the first low-speed ball milling at a speed of 170r / min and a ball milling time of 24h.

[0071] The powder after the first ball milling was dried in a forced air oven at 80°C for 24 h, then ground in a mortar, passed through a 120-mesh standard sieve, and then pre-calcined at 1200°C for 4 h.

[0072] The pre-sintered powder was ground, passed through a 200-mesh standard sieve, and put into the ball mill again. ZrO2 ball milling beads with a diameter of 3 mm and deionized water were added for the second ball milling. The ball milling speed was 300 r / min and the ball milling time was 12 h.

[0073] The powder after the second ball milling was dried at 80°C for 24h, passed through a 200-mesh standard sieve, put into a granulator for granulation (1% PVA solution by mass), passed through an 80-mesh standard sieve, and finally sintered at 1450°C for 3h. After crushing, the powder was screened to obtain a granule with the chemical formula of Mg 1.99 Ga 0.01 Si 0.99 Al 0.01 O4, ceramics with a particle size of 26μm-28μm, and the mass fraction of MgSiO3 impurity phase in the ceramics is 0.5%.

[0074] Comparative Example 2 MgO, Ga2O3, Al2O3 and SiO2 with a purity of 99.99% and a particle size of 5μm are used as raw materials, prepared in a molar ratio of Mg:Ga:Si:Al of 1.99:0.01:0.99:0.01 and placed in a ball mill filled with ZrO2 ball milling beads with a diameter of 3mm. Deionized water is added to the ball mill for the first low-speed ball milling at a speed of 170r / min and a ball milling time of 24h.

[0075] The powder after the first ball milling was dried in a forced air oven at 80°C for 24 h, then ground in a mortar, passed through a 120-mesh standard sieve, and then pre-calcined at 1200°C for 4 h.

[0076] The pre-sintered powder was ground, passed through a 200-mesh standard sieve, and put into the ball mill again. ZrO2 ball milling beads with a diameter of 3 mm and deionized water were added for the second ball milling. The ball milling speed was 300 r / min and the ball milling time was 12 h.

[0077] The powder after the second ball milling was dried at 80°C for 24h, passed through a 200-mesh standard sieve, put into a granulator for granulation (1% PVA solution by mass), passed through an 80-mesh standard sieve, and finally sintered at 1450°C for 3h. After crushing, the powder was screened to obtain a granule with the chemical formula of Mg 1.99 Ga 0.01 Si 0.99 Al 0.01 O4, ceramics with a particle size of 17μm-19μm, and the mass fraction of MgSiO3 impurity phase in the ceramics is 0.4%.

[0078] Comparative Example 3 MgO, Ga2O3, Al2O3 and SiO2 with a purity of 99.99% and a particle size of 5 μm are used as raw materials, prepared in a molar ratio of Mg:Ga:Si:Al of 1.955:0.045:0.955:0.045 and placed in a ball mill filled with ZrO2 ball milling beads with a diameter of 3 mm. Deionized water is added to the ball mill for the first low-speed ball milling at a speed of 170 r / min for 24 h.

[0079] The powder after the first ball milling was dried in a forced air oven at 80°C for 24 h, then ground in a mortar, passed through a 120-mesh standard sieve, and then pre-calcined at 1200°C for 4 h.

[0080] The pre-sintered powder was ground, passed through a 200-mesh standard sieve, and put into the ball mill again. ZrO2 ball milling beads with a diameter of 3 mm and deionized water were added for the second ball milling. The ball milling speed was 300 r / min and the ball milling time was 12 h.

[0081] The powder after the second ball milling was dried at 80°C for 24h, passed through a 200-mesh standard sieve, put into a granulator for granulation (1% PVA solution by mass), passed through an 80-mesh standard sieve, and finally sintered at 1450°C for 3h. After crushing, the powder was screened to obtain a granule with the chemical formula of Mg 1.955 Ga 0.045 Si 0.955 Al 0.045 O4, a ceramic with a particle size of 56μm-58μm, and the mass fraction of MgSiO3 impurity phase in the ceramic is 0.4%.

[0082] Comparative Example 4 MgO, Ga2O3, Al2O3 and SiO2 with a purity of 99.99% and a particle size of 5 μm are used as raw materials, prepared in a molar ratio of Mg:Ga:Si:Al of 1.94:0.06:0.94:0.06 and placed in a ball mill filled with ZrO2 ball milling beads with a diameter of 3 mm. Deionized water is added to the ball mill for the first low-speed ball milling at a speed of 170 r / min and a ball milling time of 24 h.

[0083] The powder after the first ball milling was dried in a forced air oven at 80°C for 24 h, then ground in a mortar, passed through a 120-mesh standard sieve, and then pre-calcined at 1200°C for 4 h.

[0084] The pre-sintered powder was ground, passed through a 200-mesh standard sieve, and put into the ball mill again. ZrO2 ball milling beads with a diameter of 3 mm and deionized water were added for the second ball milling. The ball milling speed was 300 r / min and the ball milling time was 12 h.

[0085] The powder after the second ball milling was dried at 80°C for 24h, passed through a 200-mesh standard sieve, put into a granulator for granulation (1% PVA solution by mass), passed through an 80-mesh standard sieve, and finally sintered at 1450°C for 3h. After crushing, the powder was screened to obtain a granule with the chemical formula of Mg 1.94 Ga 0.06 Si 0.94 Al 0.06 O4, a ceramic with a particle size of 50μm-55μm, and the mass fraction of MgSiO3 impurity phase in the ceramic is 0.9%.

[0086] Application Example 1 The pH of a mixture of ethanol and water (mass ratio 1:9) was adjusted to 4 using glacial acetic acid. To 120 parts by weight of the mixture were added 60 parts by weight of the ceramic prepared in Example 1 and 1.8 parts by weight of a KH550 coupling agent at 55° C. The mixture was dispersed and dried at 80° C. for 24 h to obtain a modified ceramic.

[0087] The modified ceramic and 40 parts by weight of polytetrafluoroethylene were mixed in 80 parts by weight of deionized water solvent to obtain a resin composition.

[0088] The resin composition was impregnated on 106 glass fiber cloth and dried in an oven at 80°C for 10 minutes to obtain a semi-cured sheet. Four semi-cured sheets were stacked, and a 1oz copper foil was covered on the upper and lower surfaces respectively. The sheets were placed in a vacuum hot press and hot pressed for 8 hours at a pressure of 6MPa and a temperature of 390°C to obtain a circuit substrate.

[0089] Application Example 2 The difference between Application Example 2 and Application Example 1 is that the ceramic prepared in Example 2 is used to prepare the circuit substrate.

[0090] Application Example 3 The only difference between Application Example 3 and Application Example 1 is that the ceramic prepared in Example 3 is used to prepare the circuit substrate.

[0091] Application Example 4 The only difference between Application Example 4 and Application Example 1 is that the ceramic prepared in Example 4 is used to prepare the circuit substrate.

[0092] Application Example 5 The only difference between Application Example 5 and Application Example 1 is that the ceramic prepared in Example 5 is used to prepare the circuit substrate.

[0093] Application Example 6 The only difference between Application Example 6 and Application Example 1 is that the ceramic prepared in Example 6 is used to prepare the circuit substrate.

[0094] Application Example 7 The only difference between Application Example 7 and Application Example 1 is that the ceramic prepared in Example 7 is used to prepare the circuit substrate.

[0095] Application Example 8 The only difference between Application Example 8 and Application Example 1 is that the ceramic prepared in Example 8 is used to prepare the circuit substrate.

[0096] Application Example 9 The only difference between Application Example 9 and Application Example 1 is that the ceramic is not modified.

[0097] Application Example 10 The difference between Application Example 10 and Application Example 1 is that 50 parts by weight of the modified ceramic in Application Example 1 and 50 parts by weight of polytetrafluoroethylene are used.

[0098] Application Example 11 The difference between Application Example 11 and Application Example 1 is that 40 parts by weight of the modified ceramic in Application Example 1 and 60 parts by weight of polytetrafluoroethylene are used.

[0099] Application Example 12 The difference between Application Example 12 and Application Example 1 is that 30 parts by weight of the modified ceramic in Application Example 1 and 70 parts by weight of polytetrafluoroethylene are used.

[0100] Application Comparative Example 1 Application Example 1 is compared with Application Example 1, except that the ceramic prepared in Comparative Example 1 is used to prepare the circuit substrate.

[0101] Application Comparative Example 2 The difference between Application Example 2 and Application Example 1 is that the ceramic prepared in Comparative Example 2 is used to prepare the circuit substrate.

[0102] Application Comparative Example 3 The only difference between Application Example 3 and Application Example 1 is that the ceramic prepared in Comparative Example 3 is used to prepare the circuit substrate.

[0103] Application Comparative Example 4 The only difference between Application Example 4 and Application Example 1 is that the ceramic prepared in Comparative Example 4 is used to prepare the circuit substrate.

[0104] The performance tests were performed on the ceramics prepared in Examples 1 to 8 and Comparative Examples 1 to 4, respectively. The test results are shown in Table 1, wherein the specific test methods are as follows: Dielectric loss: using metal cavity resonance method, frequency is 10GHz; Thermal conductivity: measured using ASTM-D5470; Table 1

[0105] The performance tests were performed on the circuit substrates prepared in Application Examples 1 to 12 and Application Comparative Examples 1 to 4, respectively. The test results are shown in Table 2, wherein the specific test methods are as follows: Dielectric loss: measured using IPC-TM-650 2.5.5.5; Thermal conductivity: measured using ASTM-D5470.

[0106] Table 2

[0107] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0108] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A ceramic, characterized in that: The chemical formula of the ceramic is Mg 2-x Ga x Si 1-x Al x O4, wherein x is the amount of ion substitution, 0<x≤0.05, and when 0<x≤0.04, the particle size of the ceramic is (10+1000x)μm to (15+1000x)μm, and when 0.04<x≤0.05, the particle size of the ceramic is 50μm to 55μm.

2. The ceramic according to claim 1, characterized in that The mass fraction of the MgSiO3 impurity phase in the ceramic is less than or equal to 1%.

3. The ceramic according to claim 1, characterized in that x>0.02。 4. A method for preparing a ceramic according to any one of claims 1 to 3, characterized in that: The following steps are involved: MgO, Ga2O3, Al2O3 and SiO2 are mixed as raw materials, wherein the molar ratio of Mg, Ga, Si and Al in the raw materials is 2-x:x:1-x:x, and 0<x≤0.05; The raw material is subjected to a first ball milling to obtain a first ball milled powder; Drying, grinding, sieving and pre-calcining the powder after the first ball milling to obtain a pre-calcined powder; Grinding and sieving the pre-sintered powder again, and ball milling the powder for a second time to obtain a second ball milled powder; The powder after the second ball milling is dried, and subjected to the first screening, granulation, the second screening, sintering, crushing and screening to obtain the ceramic.

5. The method for preparing ceramics according to claim 4, characterized in that: The method for preparing the ceramic satisfies at least one of the following conditions: (1) The purity of the raw materials is above 99.5% and the particle size is below 20 μm; (2) The first ball milling uses ball milling beads with a particle size of 2 mm to 5 mm, and the solvent used includes at least one of deionized water or ethanol; (3) The second ball milling uses ball milling beads with a particle size of 2 mm-5 mm, and the solvent used includes at least one of deionized water or ethanol.

6. A resin composition, characterized in that The method comprises a resin and the ceramic according to any one of claims 1 to 3.

7. The resin composition according to claim 6, characterized in that The resin composition satisfies at least one of the following conditions: (1) The resin includes at least one of fluorine-containing resin, epoxy resin, hydrocarbon resin or polyphenylene ether resin; (2) The mass of the ceramic is 30%-70% of the total mass of the resin and the ceramic.

8. A prepreg made from the resin composition according to any one of claim 6 or claim 7.

9. A circuit substrate made of the prepreg as claimed in claim 8.

10. A printed circuit board made using the circuit substrate as claimed in claim 9.

Citation Information

Patent Citations

  • Spherical forsterite particles, method for producing same, and resin composition including spherical forsterite particles

    CN113165888A

  • Prepreg, circuit substrate and printed circuit board

    CN116162342A

  • Dielectric porcelain composition for high frequency and dielectric resonator

    JP1998017360A

  • Circuit board and method for manufacturing the same

    JP2016213410A