Trans-wide-band-gap perovskite thin film preparation method and solar cell
Through organic solvent-assisted pre-annealing and two-step annealing treatment, the problem of small grain size in wide-bandgap perovskite solar cells is solved, and the photoelectric performance and solar cell efficiency of the perovskite film are improved.
Patent Information
- Application Number
- CN202411103834.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-19
AI Technical Summary
In the early stage of crystal growth, wide-bandgap perovskite solar cells have weak force between PbBr2 and organic solvents, making it difficult to form a continuous mesophase, resulting in small and discontinuous grain size, affecting photoelectric performance.
The organic solvent-assisted pre-annealing method is adopted to form a stable mesophase and reduce the crystallization density by inverted pre-annealing and two-step annealing treatment, and obtain a perovskite film with larger grain size and higher purity.
The photoelectric performance and efficiency of wide-bandgap perovskite solar cells are significantly improved, the composite center and defects are reduced, and the efficiency of perovskite crystalline silicon stacked batteries is improved.
Smart Images

Figure CN118984634A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new energy photovoltaic power generation, and specifically relates to a method for preparing an inverse wide bandgap perovskite film and a solar cell. Background Art
[0002] With the rapid development of science and technology and industry, in order to achieve sustainable development, we need to find more efficient, clean and economical renewable energy. Among many renewable energy sources, solar energy has the advantages of huge reserves, wide distribution and inexhaustible supply. Solar cells use solar energy in the form of photoelectric conversion and are considered to be the most effective way to use solar energy.
[0003] As the most important part of solar cells, the light absorption layer material has always been a hot topic in the research of photovoltaic materials. Organic-inorganic metal halide perovskite (PVK) materials have the advantages of high light absorption coefficient, adjustable bandgap width, and high defect tolerance. Since it was first proposed in 2009, perovskite solar cells have developed rapidly. At present, the efficiency of a single cell exceeds 26.1%, which is close to the efficiency record of single-crystal silicon.
[0004] According to the deposition order of the carrier transport layer, perovskite solar cells can be divided into formal (nip) and trans (pin) structures. The trans structure has the advantages of low hysteresis effect and low preparation cost, and has great development potential. In addition, the trans wide-bandgap perovskite solar cells are suitable for assembly into stacked cells with TOPCon, HJT and other n-type silicon-based crystalline silicon solar cells. Perovskite crystalline silicon stacked cells using trans wide-bandgap perovskite solar cells are regarded as an effective way to break through the efficiency limit of single-junction solar cells, and the current efficiency has exceeded 33%.
[0005] Compared with narrow-bandgap perovskites without Br, wide-bandgap perovskite halogens are mainly composed of I and Br. 2 The interaction force with organic solvents such as DMSO, GBL, and NMP is relatively 2 It is weak and difficult to form PbBr in the early stage of perovskite crystal growth. 2 The continuous intermediate phase formed by complexation with the organic solvent component easily leads to the formation of perovskite grains that are smaller and discontinuous, which has an adverse effect on the photoelectric properties of perovskite. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing an inverted wide-bandgap perovskite film and a solar cell, which can effectively increase the grain size of the wide-bandgap perovskite film through an organic solvent-assisted pre-annealing, thereby improving the photoelectric performance of the wide-bandgap perovskite solar cell.
[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0008] A method for preparing an inverse wide bandgap perovskite film, comprising:
[0009] Step 1), at least one of CsI, CsBr, and FAI is mixed with PbBr 2 Dissolved in a mixed solvent consisting of DMF and organic solvent A to obtain a composition of Cs x FA 1-x PbI 3-y Br y The perovskite precursor solution has a concentration of 1.2 to 1.5 mol / L, wherein 0≤x≤1, 0.4≤y≤3, and PbI is added during dissolution according to the composition of the components. 2 、PbCl 2 , MACl or more;
[0010] Step 2), depositing a perovskite precursor solution on the surface of the hole transport layer to obtain a perovskite prefabricated layer;
[0011] Step 3), the perovskite prefabricated layer film obtained in step 2) is placed face down on a hot stage 0.5 to 1 cm above a weighing paper moistened with organic solvent A for inverted pre-annealing, and then placed face up on a hot stage for a second annealing step.
[0012] Preferably, the organic solvent A used for preparing the solution and wetting the weighing paper is one of DMSO, GBL and NMP.
[0013] Preferably, the perovskite precursor solution is deposited by one of spin coating, slit coating, doctor blade coating and screen printing.
[0014] Preferably, the thickness of the perovskite prefabricated layer is 400-800 nm.
[0015] Preferably, the inversion pre-annealing temperature is 60-80° C., and the time is 10-30 seconds.
[0016] Preferably, the second step annealing temperature is 100-150° C. and the time is 10-30 min.
[0017] An inverted wide band gap perovskite solar cell, wherein the wide band gap perovskite film prepared by any of the above methods is used as a light absorption layer, and the solar cell device structure is: indium tin oxide / hole transport layer / Cs x FA 1-x PbI 3-y Br y / electron transport layer / buffer layer / Ag.
[0018] Preferably, the hole transport layer is one of nickel oxide and poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine].
[0019] Preferably, the electron transport layer is one of [6,6]-phenyl-C61-butyric acid isomethyl ester and fullerene.
[0020] Preferably, the buffer layer is one of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline and tin dioxide.
[0021] A method for preparing an inverted wide bandgap perovskite solar cell comprises the following steps:
[0022] Step 1), treating the cleaned indium tin oxide conductive glass with ozone;
[0023] Step 2), depositing a hole transport layer on the surface of the indium tin oxide conductive glass and then heating and annealing.
[0024] Step 3), preparing a wide bandgap perovskite film on the surface of the hole transport layer by any of the methods described above;
[0025] Step 4), depositing an electron transport layer and a buffer layer on the surface of the perovskite film in sequence;
[0026] Step 5), thermally evaporate Ag on the surface of the buffer layer to construct a top electrode.
[0027] The present invention uses an organic solvent to assist in inverted pre-annealing to prepare a wide-bandgap perovskite film, which helps to form a stable intermediate phase in the early stage of perovskite crystal growth. At the same time, the organic solvent helps to dissolve the perovskite grain boundaries and reduce the perovskite crystal density. The combined effect of the two helps to obtain a perovskite film with a larger grain size and higher purity. The present invention uses a two-step annealing process of first low temperature and then high temperature to treat the perovskite prefabricated layer, which helps to obtain a perovskite film with flatter and denser grain growth.
[0028] In summary, the present invention helps to obtain a wide-bandgap perovskite film with higher crystallinity and larger grain size, and further obtain a wide-bandgap perovskite solar cell with fewer recombination centers and defects and better photoelectric performance, which has a high reference value for improving the efficiency of wide-bandgap perovskite solar cells and perovskite crystalline silicon tandem cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Schematic diagram of the organic solvent-assisted inverted pre-annealing process of the present invention.
[0030] Figure 2 These are SEM images of wide bandgap perovskite films prepared in Comparative Example 1 and Example 1, wherein (a) is Comparative Example 1 and (b) is Example 1.
[0031] Figure 3JV diagram of wide bandgap perovskite solar cells prepared in Comparative Example 1 and Example 1, wherein device A is Comparative Example 1 and device B is Example 1. DETAILED DESCRIPTION
[0032] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention.
[0033] The present invention discloses a method for preparing an inverted wide bandgap film with improved crystallization and a solar cell. Before high-temperature annealing, low-temperature inversion pre-annealing is performed with the assistance of an organic solvent to obtain a high-quality wide bandgap perovskite film with high crystallinity and large grain size. The inverted wide bandgap perovskite solar cell assembled with the film as a light absorption layer has excellent photoelectric performance and significantly improved photoelectric conversion efficiency.
[0034] In order to have a better understanding of the present invention, the present invention will be further described by way of embodiments.
[0035] Comparative Example 1
[0036] 1) The indium tin oxide glass substrate is cleaned and then treated with ozone.
[0037] 2) Spin-coating nickel oxide on the surface of indium tin oxide conductive glass as a hole transport layer and heat annealing to a thickness of 30 nm.
[0038] 3) Prepare a wide bandgap perovskite precursor solution and mix PbI 2 、PbBr 2 , CsI, and FAI were dissolved in a mixed solvent consisting of DMF and DMSO in a stoichiometric ratio to obtain a Cs 0.1 FA 0.9 PbI 2.4 Br 0.6 The perovskite precursor solution has a perovskite concentration of 1.3 mol / L and a volume ratio of DMF to DMSO of 4:1. The surface morphology of the perovskite film after annealing is shown in the SEM. Figure 2 As shown in (a), it can be found that the perovskite layer has a small grain size and poor crystallization quality, which is not conducive to charge transport and has an adverse effect on device performance.
[0039] 4) Deposition of wide bandgap perovskite Cs in the hole transport layer 0.1 FA 0.9 PbI 2.4 Br 0.6 After the precursor solution, the perovskite surface was annealed upward, the deposition method was spin coating, the annealing temperature was 120°C, the annealing time was 25 min, and the thickness was 500 nm.
[0040] 5) An electron transport layer and a buffer layer are sequentially deposited on the surface of the wide bandgap perovskite film. The electron transport layer is [6,6]-phenyl-C61-butyric acid isomethyl ester with a thickness of 40 nm, and the buffer layer is 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline with a thickness of 5 nm.
[0041] 6) Ag is deposited on the surface of the buffer layer by thermal evaporation with a thickness of 80 nm.
[0042] Example 1
[0043] 1) The indium tin oxide glass substrate is cleaned and then treated with ozone.
[0044] 2) Spin-coating nickel oxide on the surface of indium tin oxide conductive glass as a hole transport layer and heat annealing to a thickness of 30 nm.
[0045] 3) Prepare a wide bandgap perovskite precursor solution and mix PbI 2 、PbBr 2 , CsI, and FAI were dissolved in a mixed solvent consisting of DMF and DMSO in a stoichiometric ratio to obtain a mixture of Cs 0.1 FA 0.9 PbI 2.4 Br 0.6 The perovskite precursor solution has a perovskite concentration of 1.3 mol / L and a volume ratio of DMF to DMSO of 4:1.
[0046] 4) Spin coating of wide bandgap perovskite Cs on the surface of the hole transport layer 0.1 FA 0.9 PbI 2.4 Br 0.6 Precursor solution, then the perovskite surface is placed on the hot stage with the DMSO wetted weighing paper facing down for inverted pre-annealing at 0.5 cm above the hot stage, the annealing temperature is 75 ° C, the time is 10 s, and then the perovskite surface is placed on the hot stage with the annealing temperature facing up, the time is 25 min, and the thickness is 500 nm. The surface morphology of the perovskite film after annealing is shown in the SEM. Figure 2 As shown in (b), it can be found that the perovskite layer has a larger grain size and better crystallization quality, which is beneficial to suppress non-radiative recombination and can optimize the device performance to a certain extent.
[0047] 5) An electron transport layer and a buffer layer are sequentially spin-coated on the surface of the wide bandgap perovskite film. The electron transport layer is [6,6]-phenyl-C61-butyric acid isomethyl ester with a thickness of 40 nm, and the buffer layer is 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline with a thickness of 5 nm.
[0048] 6) Ag is deposited on the surface of the buffer layer by thermal evaporation with a thickness of 80 nm.
[0049] 7) The JV diagrams of the perovskite solar cells prepared in Example 1 and Comparative Example 1 are as follows Figure 3 As shown, the photoelectric conversion efficiency of device A is 18.66%, and the photoelectric conversion efficiency of device B is 21.31%. It can be concluded that organic solvent-assisted pre-annealing can obtain a perovskite light absorption layer film with high crystallinity and large grain size, which helps to improve the photoelectric conversion efficiency of the device.
[0050] Example 2
[0051] 1) The indium tin oxide glass substrate is cleaned and then treated with ozone.
[0052] 2) Spin-coating nickel oxide on the surface of indium tin oxide conductive glass as a hole transport layer and heat annealing to a thickness of 30 nm.
[0053] 3) Prepare a wide bandgap perovskite precursor solution and mix PbI 2 、PbBr 2 , FAI is dissolved in a mixed solvent consisting of DMF and DMSO according to a stoichiometric ratio to obtain FAPbI 2.25 Br 0.75 The perovskite precursor solution has a perovskite concentration of 1.2 mol / L and a volume ratio of DMF to DMSO of 4:1.
[0054] 4) Spin coating of wide bandgap perovskite FAPbI on the surface of the hole transport layer 2.25 Br 0.75 Precursor liquid, then the perovskite surface is placed face down on the hot stage 0.5 cm above the DMSO-moistened weighing paper for inverted pre-annealing, the annealing temperature is 75 ° C, the time is 20 s, and then the perovskite surface is placed face up on the hot stage for annealing, the annealing temperature is 120 ° C, the time is 25 min, and the thickness is 500 nm.
[0055] 5) An electron transport layer and a buffer layer are sequentially spin-coated on the surface of the wide bandgap perovskite film. The electron transport layer is [6,6]-phenyl-C61-butyric acid isomethyl ester with a thickness of 40 nm, and the buffer layer is 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline with a thickness of 5 nm.
[0056] 6) Ag is deposited on the surface of the buffer layer by thermal evaporation with a thickness of 80 nm.
[0057] Example 3
[0058] 1) The indium tin oxide glass substrate is cleaned and then treated with ozone.
[0059] 2) Spin-coating nickel oxide on the surface of indium tin oxide conductive glass as a hole transport layer and heat annealing to a thickness of 30 nm.
[0060] 3) Prepare a wide bandgap perovskite precursor solution and mix PbI 2 、PbBr 2 , CsI, and FAI were dissolved in a mixed solvent consisting of DMF and NMP in a stoichiometric ratio to obtain a mixture of Cs 0.1 FA 0.9 PbI 2.4 Br 0.6 The perovskite precursor solution has a perovskite concentration of 1.3 mol / L and a volume ratio of DMF to NMP of 4:1.
[0061] 4) Spin coating of wide bandgap perovskite Cs on the surface of the hole transport layer 0.1 FA 0.9 PbI 2.4 Br 0.6 Precursor liquid, then the perovskite surface is placed face down on the hot stage 0.5 cm above the NMP moistened weighing paper for inverted pre-annealing, the annealing temperature is 70 ° C, the time is 20 s, and then the perovskite surface is placed face up on the hot stage for annealing, the annealing temperature is 120 ° C, the time is 25 min, and the thickness is 500 nm.
[0062] 5) An electron transport layer and a buffer layer are sequentially spin-coated on the surface of the wide bandgap perovskite film. The electron transport layer is fullerene with a thickness of 40 nm, and the buffer layer is 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline with a thickness of 5 nm.
[0063] 6) Ag is deposited on the surface of the buffer layer by thermal evaporation with a thickness of 80 nm.
[0064] Example 4
[0065] 1) The indium tin oxide glass substrate is cleaned and then treated with ozone.
[0066] 2) Spin coating poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] as a hole transport layer on the surface of indium tin oxide conductive glass and heat annealing to a thickness of 30 nm.
[0067] 3) Prepare a wide bandgap perovskite precursor solution and mix PbBr 2 , CsBr 2 Dissolved in a mixed solvent of DMF and DMSO according to a stoichiometric ratio to obtain CsPbBr 3 The perovskite precursor solution has a perovskite concentration of 1.3 mol / L and a volume ratio of DMF to DMSO of 4:1.
[0068] 4) Spin coating of wide bandgap perovskite CsPbBr on the surface of the hole transport layer 3Precursor liquid, then the perovskite surface is placed face down on the hot stage 1 cm above the DMSO-moistened weighing paper for inverted pre-annealing, the annealing temperature is 75 ° C, the time is 10 s, and then the perovskite surface is placed face up on the hot stage for annealing, the annealing temperature is 150 ° C, the time is 20 min, and the thickness is 500 nm.
[0069] 5) An electron transport layer and a buffer layer are sequentially spin-coated on the surface of the wide bandgap perovskite film. The electron transport layer is fullerene with a thickness of 40 nm, and the buffer layer is 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline with a thickness of 5 nm.
[0070] 6) Ag is deposited on the surface of the buffer layer by thermal evaporation with a thickness of 80 nm.
[0071] Example 5
[0072] 1) The indium tin oxide glass substrate is cleaned and then treated with ozone.
[0073] 2) Spin-coating nickel oxide on the surface of indium tin oxide conductive glass as a hole transport layer and heat annealing to a thickness of 30 nm.
[0074] 3) Prepare a wide bandgap perovskite precursor solution and mix PbI 2 、PbBr 2 , CsI, and FAI were dissolved in a mixed solvent consisting of DMF and GBL according to a stoichiometric ratio, and MACl, PbCl 2 As additives, MACl, PbCl 2 The amount of PbI 2 5% by mole, the composition is Cs 0.1 FA 0.9 PbI 2.4 Br 0.6 The perovskite precursor solution has a perovskite concentration of 1.3 mol / L and a volume ratio of DMF to GBL of 4:1.
[0075] 4) Spin coating of wide bandgap perovskite Cs on the surface of the hole transport layer 0.1 FA 0.9 PbI 2.4 Br 0.6 Precursor liquid, then the perovskite surface is placed on the hot stage with the GBL wetted weighing paper facing down for inverted pre-annealing 1 cm above the hot stage, the annealing temperature is 75 ° C, the time is 10s, and then the perovskite surface is placed on the hot stage for annealing with the annealing temperature of 120 ° C, the time is 25min, and the thickness is 500nm. The surface morphology of the perovskite film after annealing is shown in the SEM. Figure 2 As shown in (b), it can be found that the perovskite layer has a larger grain size and better crystallization quality, which is beneficial to suppress non-radiative recombination and can optimize the device performance to a certain extent.
[0076] 5) An electron transport layer and a buffer layer are sequentially spin-coated on the surface of the wide bandgap perovskite film. The electron transport layer is [6,6]-phenyl-C61-butyric acid isomethyl ester with a thickness of 40 nm, and the buffer layer is 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline with a thickness of 5 nm.
[0077] 6) Ag is deposited on the surface of the buffer layer by thermal evaporation with a thickness of 80 nm.
Claims
1. A method for preparing an inverse wide bandgap perovskite film, Features: The method comprises: Step 1), at least one of CsI, CsBr, and FAI is mixed with PbBr 2 Dissolved in a mixed solvent consisting of DMF and organic solvent A to obtain a composition of Cs x FA 1-x PbI 3-y Br y The perovskite precursor solution has a concentration of 1.2 to 1.5 mol / L, wherein 0≤x≤1, 0.4≤y≤3, and PbI is added during dissolution according to the composition of the components. 2 、PbCl 2 , MACl or more; Step 2), depositing a perovskite precursor solution on the surface of the hole transport layer to obtain a perovskite prefabricated layer; Step 3), the perovskite prefabricated layer film obtained in step 2) is placed face down on a hot stage 0.5 to 1 cm above a weighing paper moistened with organic solvent A for inverted pre-annealing, and then placed face up on a hot stage for a second annealing.
2. The method for preparing an inverse wide bandgap perovskite film according to claim 1, Features: The organic solvent A used for preparing the solution and wetting the weighing paper is one of DMSO, GBL and NMP.
3. The method for preparing an inverse wide bandgap perovskite film according to claim 1, Features: The perovskite precursor solution is deposited in a manner selected from the group consisting of spin coating, slit coating, scraping, and screen printing.
4. The method for preparing an inverse wide bandgap perovskite film according to claim 1, Features: The thickness of the perovskite prefabricated layer is 400-800 μm.
5. The method for preparing an inverse wide bandgap perovskite film according to claim 1, Features: The inversion pre-annealing temperature is 60-80° C., and the time is 10-30 seconds.
6. The method for preparing an inverse wide bandgap perovskite film according to claim 1, Features: The second step annealing temperature is 100-150° C. and the time is 10-30 minutes.
7. An inverted wide bandgap perovskite solar cell, Features: The wide bandgap perovskite film prepared by the method according to any one of claims 1 to 6 is used as a light absorption layer, and the solar cell device structure is: indium tin oxide / hole transport layer / Cs x FA 1-x PbI 3-y Br y / electron transport layer / buffer layer / Ag.
8. An inverted wide bandgap perovskite solar cell according to claim 7, Features: The hole transport layer is one of nickel oxide and poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine].
9. An inverted wide bandgap perovskite solar cell according to claim 7, Features: The electron transport layer is one of [6,6]-phenyl-C61-butyric acid isomethyl ester and fullerene.
10. An inverted wide bandgap perovskite solar cell according to claim 7, Features: The buffer layer is one of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline and tin dioxide.