PSN-PZT-based piezoelectric ceramic material with high mechanical quality factor and large piezoelectric coefficient and preparation method of PSN-PZT-based piezoelectric ceramic material
By using Pb1-xBax(Sb0.5Nb0.5)yZrzTi1-y-zO3-0.6mol%Mn-based material and thermoelectric coupling treatment in piezoelectric ceramic materials, the mechanical quality factor and piezoelectric coefficient of piezoelectric ceramic materials are solved. The constraint relationship of the two components of high mechanical quality factor and large piezoelectric coefficient are realized, and are suitable for high-power transducers.
Patent Information
- Application Number
- CN202410884768.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-03
AI Technical Summary
In high-power piezoelectric applications, there is a mutual restriction relationship between the mechanical quality factor and the piezoelectric coefficient of piezoelectric ceramic materials, which limits the energy loss and vibration speed of the device, affecting service life and output power.
Using Pb1-xBax(Sb0.5Nb0.5)yZrzTi1-y-zO3-0.6mol%Mn-based piezoelectric ceramic material, the MPB region of lattice distortion and multiphase coexistence is introduced through co-doping of Ba and Mn, combined with thermoelectric coupling Treatment to improve the mechanical quality factor and piezoelectric coefficient.
It achieves a combination of high mechanical quality factor and large piezoelectric coefficient, improves the electromechanical performance and temperature stability of the material, and is suitable for high-power transducers.
Smart Images

Figure CN118955128A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of piezoelectric ceramic material preparation, and specifically relates to a PSN-PZT-based piezoelectric ceramic material with high mechanical quality factor and large piezoelectric coefficient, which is mainly used for high-power transducers, and a preparation method thereof. Background Art
[0002] Piezoelectric transducers have the characteristics of high electroacoustic efficiency and large power capacity, and are widely used in modern high-tech fields such as petrochemicals, aerospace, and medical equipment. As the core component of piezoelectric transducers, PZT-based piezoelectric ceramic materials use the positive / reverse piezoelectric effect to achieve efficient conversion between mechanical energy and electrical energy. However, during the operation of the transducer, energy loss will inevitably lead to heat generation, which will directly affect the service life of the device. Therefore, piezoelectric ceramics are required to have a high mechanical quality factor to ensure that energy loss is minimized as much as possible. At the same time, in order to achieve more efficient vibration speeds and increase output power, piezoelectric ceramics need to have a large piezoelectric coefficient, which will help promote the miniaturization and intelligent development of electromechanical equipment.
[0003] For high-power piezoelectric applications, piezoelectric ceramics should not only meet the requirements of high mechanical quality factor, but also have large piezoelectric coefficient and electromechanical coupling coefficient. However, for piezoelectric ceramics, the mechanical quality factor and piezoelectric coefficient are usually mutually restrictive, which seriously limits the further development of high-power piezoelectric applications. Summary of the invention
[0004] In view of the above technical problems, the object of the present invention is to provide a PSN-PZT-based piezoelectric ceramic material having both high mechanical quality factor and large piezoelectric coefficient and a preparation method thereof.
[0005] In a first aspect, the present invention provides a PSN-PZT-based piezoelectric ceramic material, wherein the chemical composition of the PSN-PZT-based piezoelectric ceramic material is Pb 1-x Ba x (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y-z O 3 -0.6 mol% Mn; Among them: 0≤x≤0.16, 0.01≤y≤0.04, 0.50≤z≤0.52.
[0006] Preferably, the mechanical quality factor of the PSN-PZT-based piezoelectric ceramic material is at least 546, preferably 546 to 726, and more preferably 679 to 726; The piezoelectric coefficient of the PSN-PZT-based piezoelectric ceramic material is at least 423 pC / N, preferably 423 to 502 pC / N, and more preferably 474 to 502 pC / N; The Curie temperature of the PSN-PZT-based piezoelectric ceramic material is 233-350°C.
[0007] In a second aspect, the present invention provides a method for preparing the above-mentioned PSN-PZT-based piezoelectric ceramic material, the preparation method comprising the following steps: (1) According to the chemical composition ratio of the above-mentioned PSN-PZT-based piezoelectric ceramic material, weigh Pb 3 O 4 Powder, BaCO 3 Powder, Sb 2 O 3 Powder, Nb 2 O 5 Powder, ZrO 2 Powder, TiO 2 Powder, MnCO 3 Powder, after mixing, drying and sieving, raw material powder is obtained; (2) calcining and finely grinding the raw material powder to obtain ceramic powder; (3) mixing the ceramic powder with a binder, granulating, aging and molding to obtain a ceramic green body; (4) Extruding, sintering, and cooling the ceramic green body to obtain the PSN-PZT-based piezoelectric ceramic material.
[0008] Preferably, in step (1), the purity of the raw material powder is > 99%; The mixing method is ball milling, the ball milling medium is zirconium balls and water, wherein the weight ratio of material: water: ball is 0.9-1.1: 1.1-1.3: 2.5-3.5, preferably 1: 1.2: 3; the ball milling speed is 300-360 rpm, preferably 340 rpm, and the ball milling time is 3-5 hours, preferably 4 hours; The drying temperature is 80-120°C and the drying time is 6-12h; The sieve has a mesh size of 30-50, preferably 40.
[0009] Preferably, in step (2), the calcination temperature is 840-860°C, preferably 850°C, the holding time is 1-3 hours, preferably 2 hours, and the heating rate is 1-2°C / min, preferably 2°C / min; The ball milling medium for fine grinding is water and zirconium balls, the weight ratio of material: water: ball is 0.9-1.1: 1.2-1.4: 3-5, preferably 1: 1.3: 4; the ball milling speed is 350-400 rpm, preferably 360 rpm, and the ball milling time is 5-8 hours, preferably 6 hours; The particle size of the finely ground ceramic powder is controlled to be 1-3um.
[0010] Preferably, in step (3), the binder is a polyvinyl alcohol aqueous solution with a concentration of 6-7wt%; wherein the amount of the binder added is 5-7wt% of the mass of the ceramic powder, preferably 6wt%; The aging temperature is 20-30° C., and the aging time is 12-36 hours, preferably 24 hours.
[0011] Preferably, in step (4), the temperature of the plastic discharge is 600-700°C, preferably 650°C, the holding time is 1.5-3 hours, preferably 2 hours, and the heating rate is 1-2°C / min, preferably 2°C / min; The sintering temperature is 1220-1270°C, preferably 1250°C, the holding time is 1-3 hours, preferably 2 hours, and the heating rate is 1-3°C / min, preferably 2°C / min; The cooling process is: firstly cooling to 800-900°C at a rate of 1-5°C / min, preferably first cooling to 850°C at a rate of 2°C / min, and then naturally cooling to room temperature along with the furnace.
[0012] Preferably, step (4) further includes silver sintering and thermoelectric coupling treatment of the cooled blank.
[0013] Preferably, the silver-burning treatment process comprises: grinding the cooled blank to a thickness of 0.9-1.1 mm, coating silver electrodes on the upper and lower surfaces of the blank by screen printing, and then silver-burning treatment at 750-850° C. for 10-20 minutes; Preferably, the cooled blank is polished to a thickness of 1 mm, silver electrodes are coated on the upper and lower surfaces of the blank by screen printing, and then the silver is calcined at 800° C. for 15 minutes.
[0014] Preferably, the process of the thermoelectric coupling treatment includes: heating the silver-sintered blank to 290-400°C, then adjusting the voltage through a voltage regulator so that the electric field loaded on the silver-sintered blank is 100-500V / mm and remains unchanged, waiting for natural cooling to room temperature to complete the thermoelectric coupling treatment.
[0015] Beneficial Effects The Pb provided by the present invention 1-x Bax (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y-z O 3 -0.6mol% Mn piezoelectric ceramic material, through Ba and Mn co-doping to cause lattice distortion and change of phase structure, not only has excellent electromechanical properties, but also has good temperature stability and stable preparation process, and is a strong candidate material for high-power transducers. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The PSN-PZT-based piezoelectric ceramic material (Pb 1-x Ba x (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y- z O 3 -0.6mol%Mn) XRD pattern; Figure 2 The PSN-PZT-based piezoelectric ceramic material (Pb 1-x Ba x (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y- z O 3 -0.6mol%Mn) dielectric temperature spectrum curve; Figure 3 The PSN-PZT-based piezoelectric ceramic material (Pb 1-x Ba x (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y- z O 3 -0.6mol%Mn) as a function of x. DETAILED DESCRIPTION
[0017] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0018] First, the present invention provides a PSN-PZT-based piezoelectric ceramic material having both high mechanical quality factor and large piezoelectric coefficient. The chemical composition of the PSN-PZT-based piezoelectric ceramic material may be: Pb 1-x Ba x (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y-z O 3 -0.6mol%Mn(Pb 1-x Ba x SNZT-Mn); where: 0≤x≤0.16, 0.01≤y≤0.04, 0.50≤z≤0.52.
[0019] The present invention selects the ternary system PSN-PZT as the matrix material, and obtains a PZT-based piezoelectric material with a high mechanical quality factor and a large piezoelectric coefficient by replacing the Pb element at the A position of the perovskite with Ba element in an equimolar manner and doping with 0.6 mol% Mn. Among them, the high piezoelectric coefficient comes from the lattice distortion caused by Ba doping and the MPB region where multiple phases coexist; at the same time, the high orientation domain structure obtained by the thermoelectric coupling treatment leads to the enhancement of the non-intrinsic contribution of its piezoelectric response, which is also the main reason for its high piezoelectric coefficient. The high mechanical quality factor comes from the defect dipole formed by Mn doping and the additional oxygen vacancies formed in the lattice due to Ba segregation that inhibit the movement of the domain wall. In addition, the component ceramic obtained by doping with Ba and Mn elements has both a high mechanical quality factor and a large piezoelectric coefficient, and also has a high Curie temperature and good temperature stability, and is expected to be applied to the field of high-power transducers.
[0020] If the value of x is too large, the piezoelectric coefficient will increase slightly, but due to the enhancement of the diffuse phase transition effect, its mechanical quality factor and Curie temperature will be significantly reduced; if the value of y is too large or too small, or if z is too large or too small, its phase structure will shift to the MPB region where multiple phases coexist, which is not conducive to the piezoelectric coefficient. If the doping amount of Mn is too large, the defect dipole formed by it will have too strong a pinning effect on the domain wall, resulting in a decrease in the piezoelectric coefficient; and if the doping amount is too small, its mechanical quality factor is small, and it only has the performance characteristics of a high piezoelectric coefficient.
[0021] The piezoelectric coefficient of the PSN-PZT-based piezoelectric ceramic material was tested by using a ZJ-3A quasi-static tester from the Institute of Acoustics, Chinese Academy of Sciences; and the mechanical quality factor of the PSN-PZT-based piezoelectric ceramic material was tested by using an impedance analyzer (HP4294A).
[0022] In some embodiments, the mechanical quality factor of the PSN-PZT-based piezoelectric ceramic material is at least 546, preferably 546-726, and more preferably 679-726; the piezoelectric coefficient of the PSN-PZT-based piezoelectric ceramic material is at least 423pC / N, preferably 423-502pC / N, and more preferably 474-502pC / N; the Curie temperature of the PSN-PZT-based piezoelectric ceramic material is 233-350°C.
[0023] The following is an exemplary description of the preparation method of the PSN-PZT-based piezoelectric ceramic material having both high mechanical quality factor and large piezoelectric coefficient provided by the present invention. The preparation method of the PSN-PZT-based piezoelectric ceramic material may include the following steps: (1) According to Pb 1-x Ba x (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y-z O 3 -0.6mol%Mn in chemical composition ratio, weigh Pb 3 O 4 Powder, BaCO 3 Powder, Sb 2 O 3 Powder, Nb 2 O 5 Powder, ZrO 2 Powder, TiO 2 Powder, MnCO 3 Powder, after mixing, drying and sieving, raw material powder is obtained; (2) calcining and finely grinding the raw material powder to obtain ceramic powder; (3) mixing the ceramic powder with a binder, granulating, aging and molding to obtain a ceramic green body; (4) Extruding, sintering, and cooling the ceramic green body to obtain the PSN-PZT-based piezoelectric ceramic material.
[0024] In some embodiments, in step (1), the purity of the raw material powder is greater than 99%; the mixing method can be ball milling, and the ball milling medium can be zirconium balls and water, wherein the weight ratio of material: water: balls can be 0.9-1.1: 1.1-1.3: 2.5-3.5, preferably 1: 1.2: 3; the ball milling speed can be 300-360 rpm, preferably 340 rpm, and the ball milling time can be 3-5 hours, preferably 4 hours; the drying temperature can be 80-120°C, and the drying time can be 6-12 hours; the sieve can be 30-50 mesh, preferably 40 mesh.
[0025] In some embodiments, in step (2), the calcination temperature may be 840-860°C, preferably 850°C, the holding time may be 1-3 hours, preferably 2 hours, and the heating rate may be 1-2°C / min, preferably 2°C / min. The purpose of calcination is to carry out chemical reactions and synthesize a single phase. If the calcination temperature is too low, the reaction is not sufficient and the performance is reduced; if the calcination temperature is too high, it is easy to cause a large amount of lead oxide to volatilize, making it difficult to crush the pre-burned material block.
[0026] In some embodiments, in step (2), the finely ground ball milling medium may be water and zirconium balls, and the weight ratio of material: water: balls may be 0.9-1.1:1.2-1.4:3-5, preferably 1:1.3:4; the ball milling speed may be 350-400 rpm, preferably 360 rpm, and the ball milling time may be 5-8 hours, preferably 6 hours.
[0027] In some embodiments, in step (2), the particle size of the ceramic powder after fine grinding can be controlled to be 1-3um. The process of fine grinding after calcination can play the following roles: (1) Particle homogenization: The particle size of the ceramic powder after calcination is uneven, and fine grinding can break up and homogenize these particles to ensure the density and uniformity of the material during the subsequent molding and sintering process; (2) Improve sintering activity: The powder after fine grinding has a larger specific surface area, which helps to improve the activity during sintering, so that dense sintering can be achieved at a lower temperature, thereby reducing the growth of grains and improving the mechanical properties and piezoelectric properties of the material; (3) Improve molding performance: The powder after fine grinding has better fluidity and is easy to mold, which can reduce defects in the molding process, improve the density and uniformity of the green body, and thus improve the quality of the final product.
[0028] In some embodiments, in step (3), the binder may be a polyvinyl alcohol aqueous solution with a concentration of 6-7 wt %; wherein the amount of the binder added may be 5-7 wt % of the mass of the ceramic powder, preferably 6 wt %.
[0029] In some embodiments, in step (3), the aging temperature may be 20-30° C., and the aging time may be 12-36 hours, preferably 24 hours. Aging can rearrange and adjust the particles inside the material, eliminate internal stress, and thus improve the uniformity and stability of the green body.
[0030] In some embodiments, in step (4), the temperature of the extrusion molding may be 600-700°C, preferably 650°C, the holding time may be 1.5-3 hours, preferably 2 hours, and the heating rate may be 1-2°C / min, preferably 2°C / min.
[0031] In some embodiments, in step (4), the sintering temperature may be 1220-1270°C, preferably 1250°C, the holding time may be 1-3 hours, preferably 2 hours, and the heating rate may be 1-3°C / min, preferably 2°C / min. If the sintering temperature is too high or the holding time is too long, the grains may grow abnormally, resulting in abnormally large and irregularly shaped grains, and lead volatilization may be serious; if the sintering temperature is too low or the holding time is too short, the ceramic material may not be fully dense, leaving more pores, affecting the mechanical strength and piezoelectric properties of the material.
[0032] In some embodiments, in step (4), the cooling process may be: first cooling to 800-900°C (e.g. 850°C) at a rate of 1-5°C / min (e.g. 2°C / min), and then naturally cooling to room temperature in the furnace. This cooling rate may promote the segregation of Ba in the material system, forming internal defect vacancies, so as to obtain a higher mechanical quality factor.
[0033] In some embodiments, step (4) may further include silver sintering and thermoelectric coupling treatment of the cooled blank.
[0034] In some embodiments, the silver-burning process may include: grinding the cooled blank to a thickness of 0.9-1.1 mm (e.g., 1 mm), coating silver electrodes on the upper and lower surfaces of the blank by screen printing, and then silver-burning at 750-850° C. (e.g., 800° C.) for 10-20 minutes (e.g., 15 minutes).
[0035] In some embodiments, the process of the thermoelectric coupling treatment may include: heating the silver-sintered blank to 30-100°C (e.g., 290-400°C) above the Curie temperature, then adjusting the voltage through a voltage regulator so that the electric field loaded on the silver-sintered blank is 100-500V / mm (e.g., 500V / mm) and remains unchanged, waiting for natural cooling to room temperature to complete the thermoelectric coupling treatment.
[0036] If the temperature is too low (lower than the Curie temperature), the re-nucleation process of the domain structure cannot be achieved; if the temperature is too high (more than 100°C above the Curie temperature), the effect of domain structure regulation will be affected to a certain extent. At the same time, if the electric field is too small, the domain structure cannot be fully oriented; if the electric field is too large, it is easy to break through the ceramic sheet.
[0037] The present invention adopts a solid phase sintering method through the steps of batching, mixing, calcining, fine grinding, molding, plastic removal, sintering, silver sintering, thermoelectric coupling treatment, etc. to prepare a PSN-PZT-based piezoelectric ceramic material, which has a simple process flow, good repeatability, excellent material performance and easy control. At the same time, the piezoelectric ceramic material provided by the present invention has a simple composition, a high mechanical quality factor, a large piezoelectric coefficient and a high Curie temperature, and is suitable for the application field of high-power transducers.
[0038] The following examples are further cited to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are only an example within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description of this article, and are not limited to the specific values exemplified below. Unless otherwise specified in the following examples and comparative examples, Pb with a purity greater than 99% is used. 3 O 4 、BaCO 3 , Sb 2 O 3 , Nb 2 O 5 、ZrO 2 、TiO 2 、MnCO 3 The powder is batched according to the chemical formula.
[0039] Example 1
[0040] The PSN-PZT-based piezoelectric ceramic material (Pb 1-x Ba x (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y-z O 3 -0.6mol%Mn, x=0.00, y=0.02, z=0.51) comprises the following steps: (1) The weighed raw materials were placed in a nylon jar, and zirconia balls and deionized water were used as ball milling media. The raw materials were mixed in a mass ratio of raw materials: deionized water: zirconia balls = 1:1.2:3, and the mixture was fully mixed on a planetary ball mill for 4 hours; after drying, the mixture was passed through a 40-mesh sieve to obtain a raw material powder; (2) pressing the raw material powder into a cylindrical block by a press; heating the mixture to 850° C. at a heating rate of 2° C. / min in a muffle furnace, keeping the temperature for 2 hours, and then crushing the mixture through a 40-mesh sieve to obtain a ceramic pre-synthesized powder; mixing the ceramic pre-synthesized powder: deionized water: zirconium oxide balls in a mass ratio of 1:1.3:4, further fine grinding the mixture on a planetary ball mill for 6 hours, and then drying the mixture to obtain a ceramic powder; (3) adding a PVA binder to the ceramic powder to form granules, aging for 24 hours, passing through a 40-mesh sieve, and pressing under a pressure of 1.5 MPa to obtain a ceramic green body; (4) heating the ceramic blank to 650° C. at a heating rate of 2° C. / min, and keeping the temperature for 2 h to discharge the plastic; then, placing the blank in a crucible, heating it to 1250° C. at a heating rate of 2° C. / min, keeping the temperature for 2 h, and then cooling it to 850° C. at a cooling rate of 2° C. / min, and then cooling it to room temperature in the furnace; The cooled green blank was ground to a thickness of 1 mm on both sides, ultrasonically cleaned and dried, and then plated with silver electrodes by screen printing and fired at 800°C for 20 minutes. The silver-sintered blank is placed in a muffle furnace and heated to 400° C., and then the voltage is adjusted by a voltage regulator so that the electric field loaded on the silver-sintered blank is 500 V / mm and remains unchanged, and then it is allowed to cool naturally to room temperature to complete the thermoelectric coupling treatment, thereby obtaining the PSN-PZT-based piezoelectric ceramic material.
[0041] Example 2
[0042] The preparation method of the PSN-PZT-based piezoelectric ceramic material provided in this embodiment refers to that in Embodiment 1, with the main differences being: (1) x=0.04; and (2) the thermoelectric coupling treatment temperature is 370°C.
[0043] Example 3
[0044] The preparation method of the PSN-PZT-based piezoelectric ceramic material provided in this embodiment is similar to that in embodiment 1, except that: (1) x = 0.08; (2) the thermoelectric coupling treatment temperature is 340°C.
[0045] Example 4
[0046] The preparation method of the PSN-PZT-based piezoelectric ceramic material provided in this embodiment is similar to that in embodiment 1, except that: (1) x = 0.12; (2) the thermoelectric coupling treatment temperature is 320°C.
[0047] Example 5
[0048] The preparation method of the PSN-PZT-based piezoelectric ceramic material provided in this embodiment refers to that in Embodiment 1, with the main differences being: (1) x=0.16; and (2) the thermoelectric coupling treatment temperature is 290°C.
[0049] Figure 1 The PSN-PZT-based piezoelectric ceramic material (Pb 1-x Ba x (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y- z O 3 -0.6mol%Mn) XRD pattern. It can be seen from the figure that Pb 1-x Ba x (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y-z O 3 -0.6mol% Mn presents a single-phase perovskite structure. From the characteristic peak at around 45°, it can be seen that with the increase of Ba doping content, the phase structure changes from a tetragonal phase to a two-phase coexistence MPB.
[0050] Figure 2 The PSN-PZT-based piezoelectric ceramic material (Pb 1-x Ba x (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y- z O 3 The dielectric temperature spectrum curve of Ba-0.6mol% Mn). It can be seen from the figure that with the increase of Ba doping content, the dielectric peak shows a significant broadening phenomenon, which indicates the enhancement of its diffusion behavior.
[0051] Figure 3 The PSN-PZT-based piezoelectric ceramic material (Pb 1-x Ba x (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y- z O 3-0.6mol%Mn) with x. It can be seen from the figure that with the increase of Ba doping content, the mechanical quality factor and piezoelectric coefficient increase synchronously within a certain range, and the optimal value is reached at Example 4 (x=0.12), with the mechanical quality factor and piezoelectric coefficient reaching 726 and 502pC / N respectively.
[0052] Comparative Example 1
[0053] The preparation method of the PSN-PZT-based piezoelectric ceramic material provided in this comparative example refers to that in Example 1, the main differences are: (1) x=0.20; (2) the thermoelectric coupling treatment temperature is 260°C.
[0054] The piezoelectric coefficient of the ceramic material prepared in this comparative example only slightly increased, but its mechanical quality factor and Curie temperature both decreased significantly.
[0055] Comparative Example 2
[0056] The preparation method of the PSN-PZT-based piezoelectric ceramic material provided in this comparative example refers to that in Example 1, the main differences are: (1) x=0.12, and the Mn doping content is an excess of 1.4 mol%; (2) the thermoelectric coupling treatment temperature is 320°C.
[0057] The mechanical quality factor of the ceramic material prepared in this comparative example is greatly improved, but its piezoelectric coefficient is significantly reduced.
[0058] Table 1 below shows the piezoelectric and dielectric performance parameters of the piezoelectric ceramic materials prepared in Examples 1-5 and Comparative Examples 1-2: sample x <![CDATA[d 33 (pC / N)]]> <![CDATA[Q m ]]> <![CDATA[T c (℃)]]> <![CDATA[ε r ]]> <![CDATA[k p ]]> Example 1 0.00 423 582 350 1733 0.64 Example 2 0.04 449 658 320 1928 0.67 Example 3 0.08 474 679 291 2126 0.68 Example 4 0.12 502 726 267 2405 0.69 Example 5 0.16 507 546 233 2691 0.67 Comparative Example 1 0.20 514 370 203 3139 0.64 Comparative Example 2 0.12 410 1200 267 2437 0.65
[0059] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. A PSN-PZT-based piezoelectric ceramic material, characterized in that: The chemical composition of the PSN-PZT-based piezoelectric ceramic material is Pb 1-x Ba x (Sb 0.5 Nb 0.5 ) y Zr z Ti 1-y-z O3-0.6mol%Mn; Among them: 0≤x≤0.16, 0.01≤y≤0.04, 0.50≤z≤0.
52.
2. The PSN-PZT-based piezoelectric ceramic material according to claim 1, characterized in that: The mechanical quality factor of the PSN-PZT-based piezoelectric ceramic material is at least 546, preferably 546 to 726, and more preferably 679 to 726; The piezoelectric coefficient of the PSN-PZT-based piezoelectric ceramic material is at least 423 pC / N, preferably 423 to 502 pC / N, and more preferably 474 to 502 pC / N; The Curie temperature of the PSN-PZT-based piezoelectric ceramic material is 233-350°C.
3. A method for preparing the PSN-PZT-based piezoelectric ceramic material according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) Pb3O4 powder, BaCO3 powder, Sb2O3 powder, Nb2O5 powder, ZrO2 powder, TiO2 powder and MnCO3 powder are weighed respectively according to the chemical composition ratio of the above-mentioned PSN-PZT-based piezoelectric ceramic material, and raw material powders are obtained after mixing, drying and sieving; (2) calcining and finely grinding the raw material powder to obtain ceramic powder; (3) mixing the ceramic powder with a binder, granulating, aging and molding to obtain a ceramic green body; (4) Extruding, sintering, and cooling the ceramic green body to obtain the PSN-PZT-based piezoelectric ceramic material.
4. The preparation method according to claim 3, characterized in that: In step (1), the purity of the raw material powder is greater than 99%; The mixing method is ball milling, the ball milling medium is zirconium balls and water, wherein the weight ratio of material: water: ball is 0.9-1.1: 1.1-1.3: 2.5-3.5, preferably 1: 1.2: 3; the ball milling speed is 300-360 rpm, preferably 340 rpm, and the ball milling time is 3-5 hours, preferably 4 hours; The drying temperature is 80-120°C and the drying time is 6-12h; The sieve has a mesh size of 30-50, preferably 40.
5. The preparation method according to claim 3 or 4, characterized in that: In step (2), the calcination temperature is 840-860°C, preferably 850°C, the holding time is 1-3 hours, preferably 2 hours, and the heating rate is 1-2°C / min, preferably 2°C / min; The ball milling medium for fine grinding is water and zirconium balls, the weight ratio of material: water: ball is 0.9-1.1: 1.2-1.4: 3-5, preferably 1: 1.3: 4; the ball milling speed is 350-400 rpm, preferably 360 rpm, and the ball milling time is 5-8 hours, preferably 6 hours; The particle size of the finely ground ceramic powder is controlled to be 1-3um.
6. The preparation method according to any one of claims 3 to 5, characterized in that: In step (3), the binder is a polyvinyl alcohol aqueous solution with a concentration of 6-7wt%; wherein the amount of the binder added is 5-7wt% of the mass of the ceramic powder, preferably 6wt%; The aging temperature is 20-30° C., and the aging time is 12-36 hours, preferably 24 hours.
7. The preparation method according to any one of claims 3 to 6, characterized in that: In step (4), the temperature of the plastic discharge is 600-700°C, preferably 650°C, the holding time is 1.5-3 hours, preferably 2 hours, and the heating rate is 1-2°C / min, preferably 2°C / min; The sintering temperature is 1220-1270°C, preferably 1250°C, the holding time is 1-3 hours, preferably 2 hours, and the heating rate is 1-3°C / min, preferably 2°C / min; The cooling process is: firstly cooling to 800-900°C at a rate of 1-5°C / min, preferably first cooling to 850°C at a rate of 2°C / min, and then naturally cooling to room temperature along with the furnace.
8. The preparation method according to any one of claims 3 to 7, characterized in that: Step (4) also includes silver sintering and thermoelectric coupling treatment of the cooled blank.
9. The preparation method according to claim 8, characterized in that: The silver-burning treatment process includes: grinding the cooled blank to a thickness of 0.9-1.1 mm, coating silver electrodes on the upper and lower surfaces of the blank by screen printing, and then silver-burning treatment at 750-850° C. for 10-20 minutes; Preferably, the cooled blank is polished to a thickness of 1 mm, silver electrodes are coated on the upper and lower surfaces of the blank by screen printing, and then the silver is calcined at 800° C. for 15 minutes.
10. The preparation method according to claim 8, characterized in that: The process of the thermoelectric coupling treatment includes: heating the silver-sintered blank to 290-400°C, then adjusting the voltage through a voltage regulator so that the electric field loaded on the silver-sintered blank is 100-500V / mm and remains unchanged, waiting for natural cooling to room temperature to complete the thermoelectric coupling treatment.
Citation Information
Patent Citations
Piezoelectric ceramic for piezoelectric alarm and preparation method of piezoelectric ceramic
CN112430088A
PZT-Pb(Sb1 / 2Nb1 / 2) ternary system piezoelectric ceramic material as well as preparation method and application thereof
CN114075073A
Multi-element lead zirconate titanate-based pyroelectric ceramic material and preparation method thereof
CN114621008A
Mn-doped PIN-PSN-PT hard piezoelectric ceramic and preparation method thereof
CN116715523A
High-performance lead zirconate titanate-based piezoelectric ceramic and preparation method thereof
CN116768622A