Lead nickel tantalate-lead zirconate titanate ceramic with high electromechanical properties and temperature stability, preparation method and application thereof

By preparing lead nickel tantalate-lead zirconate titanate ceramics with both high electromechanical properties and temperature stability, the problem of insufficient material properties in color ultrasound probes has been solved, enabling the application of high-performance color ultrasound probes and reducing dependence on imported materials.

CN116589278BInactive Publication Date: 2024-11-12HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310420473.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In existing color ultrasound probes, piezoelectric materials cannot simultaneously possess high electromechanical performance and temperature stability, resulting in narrow bandwidth and low sensitivity of ceramic-based probes, and high-end color ultrasound equipment relies on imports.

Method used

A lead nickel tantalate-lead zirconate titanate ceramic with both high electromechanical properties and temperature stability was prepared by optimizing the ceramic composition and preparation process, using steps such as tape casting, lamination, cold isostatic pressing and high-temperature sintering, combined with BaTiO3 sheet template seed crystals and silver electrode treatment, to form a highly preferentially oriented ceramic structure.

Benefits of technology

The high electromechanical coupling coefficient of ceramics is close to that of piezoelectric single crystals, with a Curie temperature as high as 188℃, a piezoelectric constant d33 of 724pC/N, and an electromechanical coupling coefficient kt variation of less than 5%, thus solving the problem of unstable performance of traditional ceramics within the temperature range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116589278B_ABST
    Figure CN116589278B_ABST
Patent Text Reader

Abstract

A lead nickel tantalate-lead zirconate titanate ceramic with high electromechanical performance and temperature stability and its preparation method and application. The present invention belongs to the field of piezoelectric ceramics. The present invention solves the problem that it is difficult to achieve both high electromechanical performance and temperature stability of ceramics in the existing color Doppler ultrasound probe applications. The ceramic chemical formula of the present invention is: 0.24Pb(Ni 1 / 3Ta 2 / 3 )O3-0.33PbZrO3-0.43PbTiO3. The ceramic of the present invention is <001> The oriented barium titanate template was prepared by tape casting. The obtained ceramic has the best comprehensive performance. At this time, the ceramic piezoelectric coefficient d 33 Up to 724pC / N, Curie temperature T C The performance variation is less than 5% within the temperature range of 25-75℃, and the electromechanical coupling coefficient k t , can reach 0.57, which is close to that of piezoelectric single crystal. The introduction of lead nickel tantalate solves the serious problem of template solid solution in current high lead zirconate content (>30%) ceramics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of piezoelectric ceramics, and in particular relates to a lead nickel tantalate-lead zirconate titanate ceramic having high electromechanical properties and temperature stability, and a preparation method and application thereof. Background Art

[0002] Ultrasonic medical imaging equipment is the medical imaging equipment with the largest number of equipment and the largest number of people tested in my country. Among them, color Doppler ultrasound detector (color ultrasound) is the most widely used ultrasonic medical imaging equipment, occupying a major market share. Against the backdrop of an aging population, increased health awareness among residents, and new medical infrastructure policies, the demand for color ultrasound equipment is increasing. However, domestic color ultrasound equipment is currently in the middle and lower reaches of the industry, and high-end color ultrasound equipment and most of its components still rely on imports, and there is still a large gap between relevant scientific research accumulation and that of foreign countries. As the core component of the color ultrasound probe, piezoelectric materials are not only expected to have high electromechanical coupling coefficients and piezoelectric coefficients, but also need to have excellent temperature stability within a certain temperature range.

[0003] At present, lead-based piezoelectric ceramics and piezoelectric single crystals are the most commonly used piezoelectric materials in color Doppler ultrasound probes. Traditional piezoelectric ceramics have the advantages of low cost, low processing difficulty and excellent mechanical properties, but their poor electromechanical properties lead to narrow bandwidth and low sensitivity in ceramic-based probes, so they are mainly used in mid- and low-end color Doppler ultrasound probes. Piezoelectric single crystals are the piezoelectric materials with the best electromechanical properties and are key components in high-end color Doppler ultrasound probes. Compared with piezoelectric ceramics, the price of piezoelectric single crystals is dozens of times that of piezoelectric ceramics, and as the size increases, the difficulty of preparation increases accordingly. Summary of the invention

[0004] In order to overcome the deficiencies of the prior art, the present invention provides a lead nickel tantalate-lead zirconate titanate ceramic having high electromechanical properties and temperature stability, and a preparation method and application thereof.

[0005] The purpose of the present invention is to achieve the following technical solutions:

[0006] One of the purposes of the present invention is to provide a lead nickel tantalate-lead zirconate titanate ceramic having both high electromechanical properties and temperature stability, wherein the general chemical formula of the ceramic is: 0.24Pb(Ni 1 / 3 Ta 2 / 3 )O3-0.33PbZrO3-0.43PbTiO3.

[0007] The second object of the present invention is to provide a method for preparing lead nickel tantalate-lead zirconate titanate ceramics having both high electromechanical properties and temperature stability. The method for preparing lead nickel tantalate-lead zirconate titanate ceramics having both high electromechanical properties and temperature stability is carried out according to the following steps:

[0008] S1: 0.24Pb(Ni1 / 3 Ta 2 / 3 )O3-0.33PbZrO3-0.43PbTiO3 stoichiometric ratio, weigh PbO powder, NiO powder, Ta2O5 powder, ZrO2 and TiO2 powder, use anhydrous ethanol as ball milling medium, perform primary ball milling, drying, pre-calcination, secondary ball milling, drying in sequence, and obtain ceramic matrix powder after sieving;

[0009] S2: Mix the solvent, adhesive, plasticizer and ceramic matrix powder by ball milling for 8-12 hours, and add <001> The oriented BaTiO3 flake template seed crystals are continuously ball-milled to obtain a tape-casting slurry;

[0010] S3: preparing the tape-cast slurry into a film by tape-casting method, and then cutting, laminating, debinding, and cold isostatic pressing the film to obtain a ceramic green body;

[0011] S4: The ceramic blank is sintered at a high temperature in an air atmosphere, and then silver electrodes are coated on the upper and lower surfaces thereof, and the silver is sintered. Finally, the ceramic blank is polarized in silicone oil to obtain a lead nickel tantalate-lead zirconate titanate ceramic having high electromechanical properties and temperature stability.

[0012] It is further defined that the particle size of ZrO2 and TiO2 powders in S1 is ≤200nm.

[0013] It is further defined that the average particle size of the ceramic matrix powder obtained in S1 is below 500 nm.

[0014] It is further defined that the heating rate of the pre-burning in S1 is 3-5°C / min, the temperature is 700-750°C, and the heat preservation time is 2-3h.

[0015] It is further defined that the template seed crystal in S2 is a pure perovskite structure, with a diameter ≤50 μm and an aspect ratio ≥10.

[0016] It is further defined that the mass ratio of the template seed crystal to the ceramic matrix powder in S2 is (0.7-4):100.

[0017] It is further defined that the mass ratio of the ceramic matrix powder to the solvent, binder and plasticizer in S2 is 1:(0.4-1):(0.03-0.06):(0.02-0.06).

[0018] It is further defined that the stacking pressure in S3 is 100-150 MPa, and the pressure is maintained for 5-10 minutes.

[0019] It is further defined that the binder removal temperature in S3 is 500-600°C and the binder removal is carried out for 5-8 hours.

[0020] It is further defined that the cold isostatic pressing time in S3 is 10-20 minutes.

[0021] It is further defined that the high temperature sintering process of S4 is: first increase the temperature to 1000-1050℃ at a heating rate of 3-5℃ / min, keep warm for 1-2h, then increase the temperature to 1220-1280℃ at a heating rate of 1-2℃ / min, keep warm for 3-5h, then decrease the temperature to 800℃ at a cooling rate of 3-5℃ / min, and finally cool naturally to room temperature.

[0022] It is further defined that the silver sintering process in S4 is to increase the temperature to 550-600°C at a heating rate of 5-10°C / min and keep the temperature for 30-45 minutes.

[0023] It is further defined that during polarization in S4, the temperature of the silicone oil is 30-80°C and the electric field strength is 2kV / mm-4kV / mm.

[0024] The third object of the present invention is to provide a lead nickel tantalate-lead zirconate titanate ceramic having high electromechanical properties and temperature stability for use in ultrasonic testing.

[0025] A fourth object of the present invention is to provide a color ultrasound probe, which is made of the above-mentioned lead nickel tantalate-lead zirconate titanate ceramic with high electromechanical properties and temperature stability.

[0026] Compared with the prior art, the present invention has the following significant effects:

[0027] The present invention solves the problem that it is difficult to achieve both high electromechanical performance and temperature stability of ceramics in existing color Doppler ultrasound probe applications by optimizing ceramic components and improving the preparation process. The obtained ceramics have excellent comprehensive performance, and the specific advantages are as follows:

[0028] (1) Based on the performance requirements of piezoelectric materials in color Doppler ultrasound probes, the ceramics prepared in this invention have both high electromechanical properties and excellent temperature stability. The ceramic Curie temperature T C Up to 188℃ simultaneous piezoelectric constant d 33 It can reach 724pC / N, and has no rhombohedral-tetragonal phase transition temperature, far exceeding traditional non-oriented ceramics. In addition, the electromechanical coupling coefficient kt is close to that of piezoelectric single crystals, reaching 0.57, and the performance parameter change from room temperature to 75°C is less than 5%.

[0029] (2) The ceramic preparation method of the present invention does not require the preparation of precursors, is not prone to the appearance of pyrochlore phase, has loose sintering conditions, and has an electromechanical coupling coefficient far exceeding that of traditional ceramics and close to that of piezoelectric single crystals. The introduction of lead nickel tantalate solves the problem of the difficulty in texturing ceramics with a high lead zirconate content (>30%). BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is an X-ray diffraction pattern of lead nickel tantalate-lead zirconate titanate ceramics prepared in Example 1 and Comparative Examples 1-2 of the present invention;

[0031] Figure 2 is a surface microscopic morphology of the lead nickel tantalate-lead zirconate titanate ceramic prepared in Example 1;

[0032] Figure 3 1 is a dielectric constant thermogram of lead nickel tantalate-lead zirconate titanate ceramics prepared in Example 1 and Comparative Examples 1-2 of the present invention;

[0033] Figure 4 1 is the polarization intensity-electric field curve of the lead nickel tantalate-lead zirconate titanate ceramics prepared in Example 1 of the present invention and Comparative Examples 1-2. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0035] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.

[0036] The terms "comprising," "including," "having," "containing," or any other variations thereof, as used in the following examples, are intended to cover a non-exclusive inclusion. For example, a composition, step, method, article, or apparatus comprising the listed elements is not necessarily limited to only those elements, but may include other elements not expressly listed or inherent to such composition, step, method, article, or apparatus.

[0037] When equivalent, concentration or other value or parameter is represented by the range limited by range, preferred range or a series of upper preferred value and lower preferred value, this should be understood as specifically disclosing all ranges formed by any pairing of any upper range limit or preferred value and any lower range limit or preferred value, regardless of whether the scope is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the scope is intended to include its end value and all integers and fractions within the scope. In the present application specification and claims, range limitation can be combined and / or interchanged, if these ranges are not otherwise stated, include all sub-ranges contained therein.

[0038] The indefinite articles "a" and "an" before the elements or components of the present invention have no limitation on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the quantity obviously refers to the singular form only.

[0039] The "one embodiment" or "embodiment" of the present invention refers to a specific feature, structure or characteristic that can be included in at least one implementation of the present invention. The "in one embodiment" that appears in different places in this specification does not refer to the same embodiment, nor is it a separate or selective embodiment that is mutually exclusive with other embodiments.

[0040] Embodiment 1:

[0041] The preparation method of a lead nickel tantalate-lead zirconate titanate ceramic having high electromechanical properties and temperature stability in this embodiment is carried out by the following steps:

[0042] S1

[0043] Weighing: The target ceramic component chemical formula is 0.24Pb(Ni 1 / 3 Ta 2 / 3 )O3-0.33PbZrO3-0.43PbTiO3 as the basis, weigh PbO powder, NiO powder, Ta2O5 powder, ZrO2 and TiO2 powder as raw materials, wherein the average particle size of ZrO2 powder is ≤100nm, and the average particle size of TiO2 powder is ≤100nm;

[0044] Ball milling: add the weighed raw material powder to the ball milling medium anhydrous ethanol, ball mill for 24 hours, dry in an oven at 80°C, place in a muffle furnace after drying, heat up to 720°C at a rate of 3°C / min and keep warm for 2 hours, pre-sinter and ball mill again for 24 hours, dry in an oven at 80°C, and finally sieve with an 80-mesh sieve to obtain 20g of ceramic matrix powder with a particle size of 300nm-400nm;

[0045] S2:

[0046] Preparation of tape casting slurry: using ethanol-xylene mixed solution as solvent, polyvinyl butyral as binder, and dioctyl phthalate as plasticizer, taking 6g of solvent, weighing 0.6g of binder, 0.4g of plasticizer, and ball milling with 20g of ceramic matrix powder for 10h, then adding 0.35g of BaTiO3 flake template seed crystals with preferred orientation along <001>, diameter of 10μm, and thickness of 1μm, and continuing ball milling for 40min to obtain tape casting slurry;

[0047] S3:

[0048] Tape casting: The tape casting slurry is prepared into a film with a thickness of 240 μm by tape casting, and then cut;

[0049] Lamination: stack the cut membranes to a thickness of 1 mm and maintain the pressure at 150 MPa for 10 minutes for lamination;

[0050] Debinding: After lamination, place in a muffle furnace and debind at 550℃ for 6h;

[0051] Cold isostatic pressing: After debinding, cold isostatic pressing is performed at a pressure of 250 MPa, and the pressure is maintained for 15 minutes to obtain a ceramic green body;

[0052] S4:

[0053] High temperature sintering: Place the obtained ceramic blank in a high temperature furnace, in an air atmosphere, heat it to 1050°C at a rate of 4°C / min, keep it at that temperature for 1.5 hours, then heat it to 1260°C at a rate of 2°C / min, keep it at that temperature for 5 hours, and after the heat preservation, cool it down to 800°C at a rate of 5°C / min, and then naturally cool it to room temperature to obtain ceramics;

[0054] Silver burning: The upper and lower surfaces of the obtained ceramic are coated with silver electrodes using a screen, and then placed in a muffle furnace and heated to 550°C at a rate of 3°C / min for 30 minutes for silver burning;

[0055] Polarization: The silver-sintered ceramics were placed in 60°C silicone oil and polarized for 15 minutes at a polarization field strength of 2.5 kV / mm to obtain lead nickel tantalate-lead zirconate titanate ceramics with high electromechanical properties and temperature stability.

[0056] Comparative Example 1:

[0057] The preparation method of the lead nickel tantalate-lead zirconate titanate piezoelectric ceramic of this comparative example is carried out according to the following steps:

[0058] S1

[0059] Weighing: The target ceramic component chemical formula is 0.24Pb(Ni 1 / 3 Ta 2 / 3 )O3-0.32PbZrO3-0.44PbTiO3 as the basis, weigh PbO powder, NiO powder, Ta2O5 powder, ZrO2 and TiO2 powder as raw materials, wherein the average particle size of ZrO2 powder is ≤100nm, and the average particle size of TiO2 powder is ≤100nm;

[0060] Ball milling: add the weighed raw material powder to the ball milling medium anhydrous ethanol, ball mill for 24 hours, dry in an oven at 80°C, place in a muffle furnace after drying, heat up to 720°C at a rate of 3°C / min and keep warm for 2 hours, pre-sinter and ball mill again for 24 hours, dry in an oven at 80°C, and finally sieve with an 80-mesh sieve to obtain 20g of ceramic matrix powder with a particle size of 300nm-400nm;

[0061] S2:

[0062] Preparation of tape casting slurry: using ethanol-xylene mixed solution as solvent, polyvinyl butyral as binder, and dioctyl phthalate as plasticizer, taking 6g of solvent, weighing 0.6g of binder, 0.4g of plasticizer, and ball milling with 20g of ceramic matrix powder for 10h, then adding 0.35g of BaTiO3 flake template seed crystals with preferred orientation along <001>, diameter of 10μm, and thickness of 1μm, and continuing ball milling for 40min to obtain tape casting slurry;

[0063] S3:

[0064] Tape casting: The tape casting slurry is prepared into a film with a thickness of 240 μm by tape casting, and then cut;

[0065] Lamination: stack the cut membranes to a thickness of 1 mm and maintain the pressure at 150 MPa for 10 minutes for lamination;

[0066] Debinding: After lamination, place in a muffle furnace and debind at 550℃ for 6h;

[0067] Cold isostatic pressing: After debinding, cold isostatic pressing is performed at a pressure of 250 MPa, and the pressure is maintained for 15 minutes to obtain a ceramic green body;

[0068] S4:

[0069] High temperature sintering: Place the obtained ceramic blank in a high temperature furnace, in an air atmosphere, heat it to 1050°C at a rate of 4°C / min, keep it at that temperature for 1.5 hours, then heat it to 1260°C at a rate of 2°C / min, keep it at that temperature for 5 hours, and after the heat preservation, cool it down to 800°C at a rate of 5°C / min, and then naturally cool it to room temperature to obtain ceramics;

[0070] Silver burning: The upper and lower surfaces of the obtained ceramic are coated with silver electrodes using a screen, and then placed in a muffle furnace and heated to 550°C at a rate of 3°C / min for 30 minutes for silver burning;

[0071] Polarization: The silver-sintered ceramics were placed in 60°C silicone oil and polarized for 15 min at a polarization field strength of 2.5 kV / mm to obtain lead nickel tantalate-lead zirconate titanate ceramics.

[0072] Comparative Example 2:

[0073] The preparation method of the lead nickel tantalate-lead zirconate titanate piezoelectric ceramic of this comparative example is carried out according to the following steps:

[0074] S1

[0075] Weighing: The target ceramic component chemical formula is 0.24Pb(Ni 1 / 3 Ta 2 / 3 )O3-0.34PbZrO3-0.42PbTiO3 as the basis, weigh PbO powder, NiO powder, Ta2O5 powder, ZrO2 and TiO2 powder as raw materials, wherein the average particle size of ZrO2 powder is ≤100nm, and the average particle size of TiO2 powder is ≤100nm;

[0076] Ball milling: add the weighed raw material powder to the ball milling medium anhydrous ethanol, ball mill for 24 hours, dry in an oven at 80°C, place in a muffle furnace after drying, heat up to 720°C at a rate of 3°C / min and keep warm for 2 hours, pre-sinter and ball mill again for 24 hours, dry in an oven at 80°C, and finally sieve with an 80-mesh sieve to obtain 20g of ceramic matrix powder with a particle size of 300nm-400nm;

[0077] S2:

[0078] Preparation of tape casting slurry: using ethanol-xylene mixed solution as solvent, polyvinyl butyral as binder, and dioctyl phthalate as plasticizer, taking 6g of solvent, weighing 0.6g of binder, 0.4g of plasticizer, and ball milling with 20g of ceramic matrix powder for 10h, then adding 0.35g of BaTiO3 flake template seed crystals with preferred orientation along <001>, diameter of 10μm, and thickness of 1μm, and continuing ball milling for 40min to obtain tape casting slurry;

[0079] S3:

[0080] Tape casting: The tape casting slurry is prepared into a film with a thickness of 240 μm by tape casting, and then cut;

[0081] Lamination: stack the cut membranes to a thickness of 1 mm and maintain the pressure at 150 MPa for 10 minutes for lamination;

[0082] Debinding: After lamination, place in a muffle furnace and debind at 550℃ for 6h;

[0083] Cold isostatic pressing: After debinding, cold isostatic pressing is performed at a pressure of 250 MPa, and the pressure is maintained for 15 minutes to obtain a ceramic green body;

[0084] S4:

[0085] High temperature sintering: Place the obtained ceramic blank in a high temperature furnace, in an air atmosphere, heat it to 1050°C at a rate of 4°C / min, keep it at that temperature for 1.5 hours, then heat it to 1260°C at a rate of 2°C / min, keep it at that temperature for 5 hours, and after the heat preservation, cool it down to 800°C at a rate of 5°C / min, and then naturally cool it to room temperature to obtain ceramics;

[0086] Silver burning: The upper and lower surfaces of the obtained ceramic are coated with silver electrodes using a screen, and then placed in a muffle furnace and heated to 550°C at a rate of 3°C / min for 30 minutes for silver burning;

[0087] Polarization: The silver-sintered ceramics were placed in 60°C silicone oil and polarized for 15 min at a polarization field strength of 2.5 kV / mm to obtain lead nickel tantalate-lead zirconate titanate ceramics.

[0088] Test (1): X-ray diffraction characterization was performed on the lead nickel tantalate-lead zirconate titanate ceramics obtained in Example 1 and Comparative Examples 1-2. The results are as follows: Figure 1 As shown, from Figure 1 It can be seen that the piezoelectric textured ceramics are pure perovskite phase, and its

[001] C and

[002] C The diffraction peak intensity is much stronger than the non-<001> diffraction peak, indicating that the lead nickel tantalate-lead zirconate titanate ceramic prepared in Example 1 with both high electromechanical properties and temperature stability has a highly preferred orientation.

[0089] Test (2): The surface microstructure of the lead nickel tantalate-lead zirconate titanate ceramic prepared in Example 1 with both high electromechanical properties and temperature stability was tested. Figure 2 As shown, from Figure 2 It can be seen that the ceramic grain size is about 25 μm.

[0090] Test (3): The ceramics prepared in Example 1 and Comparative Examples 1-2 were left to stand at room temperature for 24 hours before testing their electrical properties. The dielectric constant temperature spectrum test was performed on the lead nickel tantalate-lead zirconate titanate ceramics obtained in Example 1 and Comparative Examples 1-2. The results are as follows: Figure 3 As shown in Table 1, the ferroelectric properties of the lead nickel tantalate-lead zirconate titanate ceramics obtained in Example 1 and Comparative Examples 1-2 were characterized. Figure 4 As shown in Table 1, the results show that the PE curve of the lead nickel tantalate-lead zirconate titanate ceramic with high electromechanical properties and temperature stability prepared in the embodiment of the present invention is fully saturated, and the comprehensive performance is better than that of comparative examples 1-2.

[0091] Table 1

[0092]

[0093] The above are only preferred specific embodiments of the present invention, which are all different implementations based on the overall concept of the present invention, and the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing lead nickel tantalate-lead zirconate titanate ceramics having both high electromechanical properties and temperature stability, characterized in that: Follow these steps: S1: 0.24Pb(Ni 1 / 3 Ta 2 / 3 )O3-0.33PbZrO3-0.43PbTiO3 stoichiometric ratio, weigh PbO powder, NiO powder, Ta2O5 powder, ZrO2 and TiO2 powder, use anhydrous ethanol as ball milling medium, perform primary ball milling, drying, pre-sintering, secondary ball milling, drying, and sieve to obtain ceramic matrix powder; the pre-sintering heating rate is 3-5 ℃ / min, the temperature is 700-750 ℃, and the temperature is kept for 2-3 h; S2: Mix the solvent, binder, plasticizer and ceramic matrix powder by ball milling for 8-12 hours, and add <001> The oriented BaTiO3 flake template seed crystals are continuously ball-milled to obtain a tape-casting slurry; the mass ratio of the template seed crystals to the ceramic matrix powder is (0.7-4):100, and the mass ratio of the ceramic matrix powder to the solvent, the binder, and the plasticizer is 1:(0.4-1):(0.03-0.06):(0.02-0.06); S3: preparing the tape-cast slurry into a film by tape-casting method, and then cutting, laminating, debinding, and cold isostatic pressing the film to obtain a ceramic green body; S4: The ceramic blank is sintered at high temperature in an air atmosphere, and then silver electrodes are coated on the upper and lower surfaces thereof, and the silver is sintered. Finally, it is polarized in silicone oil to obtain lead nickel tantalate-lead zirconate titanate ceramics with high electromechanical properties and temperature stability. The high-temperature sintering process is as follows: first, the temperature is increased to 1000-1050°C at a heating rate of 3-5°C / min, and kept warm for 1-2h, then the temperature is increased to 1220-1280°C at a heating rate of 1-2°C / min, and kept warm for 3-5h, then the temperature is reduced to 800°C at a cooling rate of 3-5°C / min, and finally naturally cooled to room temperature.

2. The method according to claim 1, characterized in that The template seed crystal in S2 is a pure perovskite structure with a diameter of ≤50 μm and an aspect ratio of ≥10.

3. The method according to claim 1, characterized in that In S3, the stacking pressure is 100-150 MPa, the pressure is maintained for 5-10 minutes, the binder removal temperature is 500-600 ℃, the binder removal is 5-8 hours, and the cold isostatic pressing time is 10-20 minutes.

4. The method according to claim 1, characterized in that: Silver burning process in S4: heat up to 550-600 ℃ at a rate of 5-10 ℃ / min and keep warm for 30-45 min. During polarization, the silicone oil temperature is 30-80 ℃ and the electric field strength is 2-4 kV / mm.

5. Application of lead nickel tantalate-lead zirconate titanate ceramics having high electromechanical properties and temperature stability obtained by the method described in any one of claims 1 to 4 in ultrasonic testing.