Pyrazole organic monomer, preparation method thereof, three-dimensional MOF material and application of three-dimensional MOF material
By designing the structure of dopyrazole organic ligands, the new pyrazole organic monomers are synthesized to prepare efficient MOF materials, which solves the problem of insufficient catalytic activity and stability of existing MOFs materials and achieves high efficiency for a variety of pollutants Degradation and structural stability are improved.
Patent Information
- Application Number
- CN202411029669.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The existing MOFs materials are insufficient in catalytic degradation of new pollutants, have poor stability, and are difficult to recover and reuse, making it difficult to maintain structural stability in complex environments.
Design a special dopyrazole organic ligand structure to synthesize new pyrazole organic monomers for the preparation of Ni-MOF, Zn-MOF, Mn-MOF, Co-MOF or Fe-MOF metal organic frame materials to enhance electron transfer Capacity and accessibility of reaction sites to improve catalytic activity and structural stability.
It achieves efficient degradation of various pollutants, improves the structural stability and recycling of materials, and can maintain efficient removal of heavy metals and organic pollutants in complex environments and extends service life.
Smart Images

Figure CN118955380A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic synthesis, and specifically relates to a pyrazole organic monomer and a preparation method thereof, a three-dimensional MOF material and applications thereof. Background Art
[0003] Metal-Organic Frameworks (MOFs), as a new type of porous material, have shown great potential in the fields of gas storage, separation, catalysis, etc. due to their high specific surface area, adjustable pore structure, and easy functional modification. Especially in the field of environmental pollution control, MOFs are expected to be an effective means of efficiently removing and transforming new pollutants due to their unique structure and functional diversity. However, the current MOFs materials still face some challenges in practical applications, including but not limited to: 1. Insufficient catalytic activity and universality: When existing MOFs materials catalytically degrade new pollutants, their activity and selectivity are often limited by the design of organic ligands and the selection of metal nodes, making it difficult to achieve efficient and diverse degradation of pollutants. 2. Stability issues: In actual wastewater treatment environments, MOFs may face extreme conditions such as pH changes, high temperature, and high salinity, resulting in structural damage or functional failure. 3. Difficulty in recycling and reuse: After use, MOFs materials are often difficult to effectively recycle and regenerate due to their complex structure, which increases treatment costs and environmental burdens.
[0004] In order to improve the universality, stability and regeneration performance of MOFs catalytic efficiency, a special polypyrazole organic ligand structure is designed to enhance the electron transfer ability and accessibility of reaction sites of MOFs materials, so as to achieve higher catalytic activity and selective degradation of multiple target pollutants at the same time, and keep the structure stable in complex environments, extend the service life, and reduce the frequency of maintenance and replacement. Summary of the invention
[0005] In view of the shortcomings of the above-mentioned prior art, the present invention provides a pyrazole organic monomer and a preparation method thereof, a three-dimensional MOF material and its application. The present invention synthesizes a pyrazole organic monomer with a novel structure, and uses the pyrazole organic monomer as a ligand of a three-dimensional MOF material to synthesize a Ni-MOF, Zn-MOF, Mn-MOF, Co-MOF or Fe-MOF metal organic framework material, wherein the Ni-MOF metal organic framework material can simultaneously remove multiple pollutants and heavy metal ions in water, and the Ni-MOF, Zn-MOF, Mn-MOF, Co-MOF or Fe-MOF metal organic framework material can activate PMS or H2O2 to remove organic pollutants in water.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A pyrazole organic monomer has the structural formula
[0008]
[0009] The preparation method of the pyrazole organic monomer comprises the following steps:
[0010] (1) First, 1,3,6,8-tetrabromopyrene, 1-(2-tetrahydropyranyl)pyrazole-5-boronic acid pinacol ester, tetrabutylammonium bromide and tetrakis(triphenylphosphine)palladium are placed in an alkaline organic solvent A under an inert gas atmosphere and stirred or ultrasonicated;
[0011] (2) heating under reflux in an inert gas atmosphere, cooling to room temperature, performing rotary evaporation, extraction, and rotary evaporation, adding alcohol and acid A, ultrasonication, and stirring until the acidification reaction is complete to obtain a suspension;
[0012] (3) The suspension is poured into water to adjust the pH to 7 to obtain a precipitate, which is then washed and dried to obtain a pyrazole organic monomer.
[0013] As a preferred embodiment of the present invention, the molar ratio of 1,3,6,8-tetrabromopyrene to 1-(2-tetrahydropyranyl)pyrazole-5-boric acid pinacol ester is 1:(4-8); the molar ratio of 1-(2-tetrahydropyranyl)pyrazole-5-boric acid pinacol ester to tetrabutylammonium bromide is (15-30):1; the molar ratio of 1-(2-tetrahydropyranyl)pyrazole-5-boric acid pinacol ester to tetrakis(triphenylphosphine)palladium is (60-120):1; the organic solvent A is toluene or xylene; the alkali in the alkaline organic solvent A is potassium carbonate aqueous solution, and the concentration of the potassium carbonate aqueous solution is 0.5g / mL-1.5g / mg.
[0014] The invention enhances the solubility of the substrate by using toluene or xylene, is beneficial to the contact between reactants, improves the selectivity and yield of the reaction, and inhibits the occurrence of side reactions.
[0015] As a preferred embodiment of the present invention, in the step (2), the alcohol is methanol or ethanol, and the acid A is nitric acid, hydrochloric acid or sulfuric acid; the time of the acidification reaction is 4-8 hours; the extraction liquid used in the extraction is a mixture of solvent and water, the solvent is dichloromethane or dichloroethane, and the volume ratio of the solvent to water is 1: (0.5-1); the temperature of heating reflux is 100-135°C, the time is 24-72 hours, and the heating method is oil bath or sand bath.
[0016] As a preferred embodiment of the present invention, in the step (3), the volume ratio of the suspension to water is 1:(5-10), more preferably, the volume ratio of the suspension to water is 1:(8-10).
[0017] A three-dimensional MOF material, which uses the pyrazole organic monomer as a ligand and nickel salt, zinc salt, manganese salt, cobalt salt or iron salt as a metal salt, and is prepared by a solvent thermal method to obtain a Ni-MOF metal organic framework material, a Zn-MOF metal organic framework material, a Mn-MOF metal organic framework material, a Co-MOF metal organic framework material or a Fe-MOF metal organic framework material.
[0018] As a preferred embodiment of the present invention, the method for preparing the three-dimensional MOF material, when the metal salt is a nickel salt, comprises the following steps: dissolving the pyrazole organic monomer in an organic solvent B, and then adding methanol, dimethyl sulfoxide, acid B and a nickel salt solution to obtain Ni-MOF by ultrasonication;
[0019] When the metal salt is a zinc salt, the method comprises the following steps: dissolving a pyrazole organic monomer in an organic solvent B, then adding methanol, dimethyl sulfoxide, acid C and a zinc salt solution and ultrasonically obtaining a Zn-MOF;
[0020] When the metal salt is a manganese salt, the method comprises the following steps: dissolving a pyrazole organic monomer in an organic solvent B, then adding methanol, water, acid B and a manganese salt solution and ultrasonically obtaining Mn-MOF;
[0021] When the metal salt is a cobalt salt, the method comprises the following steps: dissolving a pyrazole organic monomer in an organic solvent B, and then adding methanol, dimethyl sulfoxide, acid C and a cobalt salt solution and ultrasonically obtaining a Co-MOF;
[0022] When the metal salt is an iron salt, the method comprises the following steps: dissolving the pyrazole organic monomer in an organic solvent, then adding acetonitrile, dimethyl sulfoxide, acid B and an iron salt solution for ultrasonication, and heating the reaction to obtain Fe-MOF.
[0023] The three-dimensional MOF material prepared by the three-dimensional MOF material preparation method is a single crystal material with a clear structure.
[0024] As a preferred embodiment of the present invention, the organic solvent B is dimethyl sulfoxide, N,N-dimethylformamide or N,N-dimethylacetamide; the concentration of the pyrazole organic monomer in the organic solvent B is 5-20 mg / mL; the acid B is glacial acetic acid, and the acid C is 10% sulfuric acid; the volume ratio of the methanol, dimethyl sulfoxide, acid B and nickel salt solution is 10: (5-10): (0.7-1): (0.1-0.2); the volume ratio of methanol, dimethyl sulfoxide, acid C and zinc salt solution is 10: (5-10): (0.7-1): (0.1-0.2); The volume ratio of methyl sulfoxide, acid C and cobalt salt solution is 10: (5-10): (0.7-1): (0.1-0.2); the concentration of nickel salt solution, zinc salt solution or cobalt salt solution is 0.02 g / mL; the volume ratio of methanol, water, acid B and manganese salt solution is 10: (2-4): (0.7-1): (0.1-0.2); the concentration of manganese salt solution is 0.02 g / mL; the volume ratio of acetonitrile, dimethyl sulfoxide, acid B and iron salt solution is 10: (2-5): (0.7-1): (0.1-0.2); the concentration of iron salt solution is 0.02 g / mL.
[0025] As a preferred embodiment of the present invention, the temperature of the heating reaction is 100-140°C, the time is 12-56h, the heating rate is 10-20°C / hour, and the cooling rate is 5-10°C / hour; more preferably, the temperature of the heating reaction is 120-140°C.
[0026] The present invention also claims to protect the use of the Ni-MOF metal organic framework material in removing heavy metal ions and / or organic pollutants in sewage.
[0027] The present invention also claims to protect the use of the three-dimensional MOF material in activating PMS or H2O2 to remove organic pollutants in water.
[0028] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention synthesizes a pyrazole organic monomer compound of a new structure for the first time, and synthesizes a three-dimensional Ni-MOF, Zn-MOF, Mn-MOF, Co-MOF or Fe-MOF material based on the pyrazole organic monomer compound of the new structure by a solvent thermal method. Since the three-dimensional MOF material can produce active oxygen, the Ni-MOF material can simultaneously remove heavy metals and organic pollutants in water, and the three-dimensional MOF material can be used as an activator of PMS or H2O2 to degrade pollutants. In addition, the five MOF materials have excellent structure, performance stability, anti-interference and recyclability, and are universal for pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the mass spectrum of pyrazole organic monomer.
[0030] Figure 2 Crystal structure diagram of three-dimensional Ni-MOF material; a) coordination environment of Ni(II) in Ni-MOF, b) two-dimensional structure of Ni-MOF, c) three-dimensional structure of Ni-MOF.
[0031] Figure 3 Crystal structure diagram of three-dimensional Fe-MOF material; a) coordination environment of Fe(II) in Fe-MOF, b) three-dimensional structure of Fe-MOF-a axis, c) three-dimensional structure of Fe-MOF-b axis, d) three-dimensional structure of Fe-MOF-c axis.
[0032] Figure 4 The following are SEM images of the materials prepared in Examples 1 and 3-4. a) is a SEM image of the pyrazole organic monomer prepared in Example 1; b) is a SEM image of the three-dimensional Ni-MOF material prepared in Example 3; c) is a SEM image of the three-dimensional Fe-MOF material prepared in Example 4.
[0033] Figure 5 These are the XRD diagrams of Example 1, Example 3 and the single crystal simulated Ni-MOF material.
[0034] Figure 6 These are the XRD diagrams of Example 2, Example 4 and the single crystal simulated Fe-MOF material.
[0035] Figure 7 This is a graph showing the removal performance of the Ni-MOF prepared in Example 3 for various heavy metal ions in a mixed heavy metal system.
[0036] Figure 8 This is the adsorption isotherm of Hg(II) by Ni-MOF prepared in Example 3.
[0037] Fig. 9 This is a performance diagram of the Ni-MOF prepared in Example 3 for simultaneously removing Hg(II) and organic pollutants in different water environments.
[0038] Fig.10 The catalytic degradation effect diagram of tetracycline activated by H2O2 or PMS prepared in Example 4; a) is the catalytic degradation diagram; b) is the kinetic curve diagram.
[0039] Fig.11 a) is a diagram showing the degradation effect of Ni-MOF prepared in Example 3 on four organic pollutants; b) is a diagram showing the degradation effect of Ni-MOF prepared in Example 3 stimulating PMS on four organic pollutants.
[0040] Fig.12 This is a diagram showing the effect of Fe-MOF activating H2O2 or PMS to degrade different organic pollutants in the water of Dianchi Lake in Kunming, Yunnan. DETAILED DESCRIPTION
[0041] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0042] Example 1
[0043] A method for preparing a pyrazole organic monomer comprises the following steps:
[0044] (1) First, 4 mmol of 1,3,6,8-tetrabromopyrene was added to 140 mL of toluene under an inert gas atmosphere and stirred at room temperature for 5 minutes. Then, 25 mmol of 1-(2-tetrahydropyranyl)pyrazole-5-boronic acid pinacol ester, 0.8 g of tetrabutylammonium bromide, 150 mg of tetrakis(triphenylphosphine)palladium and 20 mL of 0.5 g / mL potassium carbonate solution were added to the reaction mixture and stirred.
[0045] (2) Reflux at 100°C for 48 hours under an inert gas atmosphere, then cool to room temperature, perform rotary evaporation under pressure at 130°C, cool to room temperature, add 100 mL of dichloromethane to dilute, pour the diluted solution into a separatory funnel, add 100 mL of water, shake and let stand for 5 minutes to remove unreacted metal catalyst and soluble impurities. After transferring the lower layer of the separatory funnel to a round-bottom flask, perform a second rotary evaporation (speed 60 r / min, temperature 40°C, under pressure). Add 100 mL of ethanol solution to the concentrated solution after the rotary evaporation, then add 20 mL of nitric acid and sonicate for 30 minutes to form an orange-yellow suspension.
[0046] (3) Pour 20 mL of the orange-yellow suspension into 200 mL of water, adjust the pH to 7 with 0.1 mol of sodium hydroxide to obtain a precipitate, wash it three times with water, and dry it to obtain a pyrazole organic monomer.
[0047] Example 2
[0048] A method for preparing a pyrazole organic monomer comprises the following steps:
[0049] (1) First, 10 mmol of 1,3,6,8-tetrabromopyrene was added to 120 mL of xylene under an inert gas atmosphere and stirred at room temperature for 2 minutes. Then, 55 mmol of 1-(2-tetrahydropyranyl)pyrazole-5-boronic acid pinacol ester, 0.6 g of tetrabutylammonium bromide, 120 mg of tetrakis(triphenylphosphine)palladium and 15 mL of 0.5 g / mL potassium carbonate solution were added to the reaction mixture and stirred.
[0050] (2) Reflux at 120°C for 48 hours under an inert gas atmosphere, then cool to room temperature, perform rotary evaporation under pressure at 150°C, cool to room temperature, add 120 mL of dichloromethane to dilute, pour the diluted solution into a separatory funnel, add 140 mL of water, shake and let stand for 5 minutes to remove unreacted metal catalyst and soluble impurities. After transferring the lower layer of the separatory funnel to a round-bottom flask, perform a second rotary evaporation (speed 60 r / min, temperature 80°C, under pressure). Add 100 mL of ethanol solution to the concentrated solution after the rotary evaporation, then add 20 mL of nitric acid and sonicate for 30 minutes to form an orange-yellow suspension.
[0051] (3) Pour 20 mL of the orange-yellow suspension into 200 mL of water, adjust the pH to 7 with 0.1 mol of sodium hydroxide to obtain a precipitate, wash it with water three times, and dry it to obtain a pyrazole organic monomer.
[0052] The mass spectra of the pyrazole organic monomers prepared in Examples 1 and 2 are as follows: Figure 1 As shown. Figure 1 It can be seen that the pyrazole organic monomer was successfully prepared, and the structural formula is
[0053]
[0054] Example 3
[0055] A method for preparing a three-dimensional Ni-MOF comprises the following steps: dissolving the pyrazole organic monomer prepared in Example 1 in N,N-dimethylformamide, preparing a 5 mg / mL solution of the pyrazole organic monomer, and ultrasonicating for 5 minutes. Taking 0.2 mL of the above solution, adding 1 mL of methanol, 0.8 mL of dimethyl sulfoxide, 0.1 mL of glacial acetic acid, and 0.1 mL, 0.02 g / mL of nickel nitrate in sequence, ultrasonicating for 10 minutes, and then reacting at 120°C for 56 hours, with a heating rate of 20°C / hour, cooling to room temperature, and a cooling rate of 5°C / hour to obtain a three-dimensional Ni-MOF material.
[0056] A method for preparing a three-dimensional Zn-MOF comprises the following steps: dissolving the pyrazole organic monomer prepared in Example 1 in N,N-dimethylformamide, preparing a 5 mg / mL solution of the pyrazole organic monomer, and ultrasonicating for 5 minutes. Take 0.2 mL of the above solution, add 1 mL of methanol, 0.8 mL of dimethyl sulfoxide, 0.1 mL0.1 mL of sulfuric acid, and 0.1 mL, 0.02 g / mL of zinc nitrate in sequence, and ultrasonicate for 10 minutes, then react at 120°C for 56 hours, with a heating rate of 20°C / hour, cool to room temperature, and cool at a rate of 5°C / hour to obtain a three-dimensional Zn-MOF material.
[0057] A method for preparing a three-dimensional Co-MOF comprises the following steps: dissolving the pyrazole organic monomer prepared in Example 1 in N,N-dimethylformamide, preparing a 5 mg / mL solution of the pyrazole organic monomer, and ultrasonicating for 5 minutes. Take 0.2 mL of the above solution, add 1 mL of methanol, 0.8 mL of dimethyl sulfoxide, 0.1 mL of glacial acetic acid (0.1 mL of sulfuric acid) and 0.1 mL, 0.02 g / mL of cobalt nitrate in sequence, and ultrasonicate for 10 minutes, then react at 120°C for 56 hours, with a heating rate of 20°C / hour, cool to room temperature, and a cooling rate of 5°C / hour to obtain a three-dimensional Co-MOF material.
[0058] A method for preparing a three-dimensional Mn-MOF material comprises the following steps: dissolving the pyrazole organic monomer prepared in Example 1 in N,N-dimethylformamide, preparing a 5 mg / mL solution of the pyrazole organic monomer, and ultrasonicating for 5 minutes. Taking 0.2 mL of the above solution, adding 1 mL of methanol, 0.4 mL of water, 0.1 mL of glacial acetic acid, and 0.1 mL, 0.02 g / mL of manganese sulfate in sequence, ultrasonicating for 5 minutes, and then reacting at 140°C for 48 hours, with a heating rate of 20°C / hour, cooling to room temperature, and a cooling rate of 5°C / hour to obtain a three-dimensional Mn-MOF material.
[0059] A method for preparing a three-dimensional Fe-MOF material comprises the following steps: dissolving the pyrazole organic monomer prepared in Example 1 in N,N-dimethylformamide, preparing a 5 mg / mL solution of the pyrazole organic monomer, and ultrasonicating for 5 minutes. Taking 0.2 mL of the above solution, adding 1 mL of acetonitrile, 0.4 mL of dimethyl sulfoxide, 0.1 mL of glacial acetic acid, and 0.1 mL, 0.02 g / mL of ferrous sulfate in sequence, ultrasonicating for 5 minutes, and then reacting at 140°C for 56 hours, with a heating rate of 20°C / hour, cooling to room temperature, and a cooling rate of 5°C / hour to obtain a three-dimensional Fe-MOF material.
[0060] Example 4
[0061] A method for preparing a three-dimensional Ni-MOF comprises the following steps: dissolving the pyrazole organic monomer prepared in Example 2 in N,N-dimethylformamide, preparing a 20 mg / mL solution of the pyrazole organic monomer, and ultrasonicating for 5 minutes. Take 0.2 mL of the above solution, add 1 mL of methanol, 0.5 mL of dimethyl sulfoxide, 0.07 mL of glacial acetic acid, and 0.2 mL, 0.02 g / mL of nickel nitrate in sequence, ultrasonicate for 10 minutes, and then react at 140°C for 12 hours, with a heating rate of 10°C / hour, cool to room temperature, and cool at a cooling rate of 5°C / hour to obtain a three-dimensional Ni-MOF material.
[0062] A method for preparing a three-dimensional Zn-MOF comprises the following steps: dissolving the pyrazole organic monomer prepared in Example 2 in N,N-dimethylformamide, preparing a 20 mg / mL solution of the pyrazole organic monomer, and ultrasonicating for 5 minutes. Take 0.2 mL of the above solution, add 1 mL of methanol, 1 mL of dimethyl sulfoxide, 0.08 mL, 0.1 mL of sulfuric acid, and 0.1 mL, 0.02 g / mL of zinc nitrate in sequence, and ultrasonicate for 10 minutes, then react at 100°C for 24 hours, with a heating rate of 15°C / hour, cool to room temperature, and cool at a rate of 5°C / hour to obtain a three-dimensional Zn-MOF material.
[0063] A method for preparing a three-dimensional Co-MOF comprises the following steps: dissolving the pyrazole organic monomer prepared in Example 2 in N,N-dimethylformamide, preparing a 5 mg / mL solution of the pyrazole organic monomer, and ultrasonicating for 5 minutes. Take 0.2 mL of the above solution, add 1 mL of methanol, 0.8 mL of dimethyl sulfoxide, 0.1 mL of glacial acetic acid (0.1 mL of sulfuric acid) and 0.1 mL, 0.02 g / mL of cobalt nitrate in sequence, and ultrasonicate for 10 minutes, then react at 120°C for 56 hours, with a heating rate of 20°C / hour, cool to room temperature, and a cooling rate of 5°C / hour to obtain a three-dimensional Co-MOF material.
[0064] A method for preparing a three-dimensional Mn-MOF material comprises the following steps: dissolving the pyrazole organic monomer prepared in Example 2 in N,N-dimethylformamide, preparing a 20 mg / mL solution of the pyrazole organic monomer, and ultrasonicating for 5 minutes. Take 0.2 mL of the above solution, add 1 mL of methanol, 0.4 mL of water, 0.1 mL of glacial acetic acid, and 0.1 mL, 0.02 g / mL of manganese sulfate in sequence, and ultrasonicate for 5 minutes, then react at 120°C for 12 hours, with a heating rate of 20°C / hour, cool to room temperature, and cool at a rate of 5°C / hour to obtain a three-dimensional Mn-MOF material.
[0065] A method for preparing a three-dimensional Fe-MOF material comprises the following steps: dissolving the pyrazole organic monomer prepared in Example 2 in N,N-dimethylformamide, preparing a 10 mg / mL solution of the pyrazole organic monomer, and ultrasonicating for 5 minutes. Take 0.2 mL of the above solution, add 1 mL of acetonitrile, 0.4 mL of dimethyl sulfoxide, 0.1 mL of glacial acetic acid, and 0.1 mL, 0.02 g / mL of ferrous sulfate in sequence, and ultrasonicate for 5 minutes, then react at 120°C for 12 hours, with a heating rate of 20°C / hour, cool to room temperature, and cool at a rate of 10°C / hour to obtain a three-dimensional Fe-MOF material.
[0066] The crystal structures of the Ni-MOF and Fe-MOF metal organic frameworks synthesized in Examples 3 and 4 are shown in Figure 2 and 3As shown in the scanning electron microscope photos Figure 4 .according to Figure 5 and 6 From the XRD analysis, it can be seen that the XRD of Ni-MOF is simulated according to the single crystal structure, and it can be seen that the synthesized Ni-MOF powder has obvious peaks at 8.98°, 10.58°, 14.58°, 18.04°, 22.16° and 24.02°; in addition, the XRD of Fe-MOF is simulated according to the single crystal structure, and it can be seen that the synthesized Ni-MOF powder has obvious peaks at 9.04°, 10.48°, 14.76°, 18.34°, 20.56° and 22.40°, and the synthesized Ni-MOF and Fe-MOF powders have high crystallinity.
[0067] Effect Example 1
[0068] Test samples: Comparative MOF (Ni-MOF two-dimensional structure) materials and materials prepared in Examples 1-4.
[0069] The preparation method of the comparative MOF comprises the following steps: A preparation method of a three-dimensional Ni-MOF material comprises the following steps: dissolving the pyrazole organic monomer prepared in Example 1 in N,N-dimethylformamide, the concentration of the pyrazole organic monomer is prepared as 10 mg / mL solution, and ultrasonicating for 5 minutes. Take 0.2 mL of the above solution, add 1 mL of methanol, 0.1 mL of glacial acetic acid and 0.1 mL, 0.02 g / mL nickel nitrate in sequence, and ultrasonicate for 10 minutes to obtain a comparative MOF material, which is a two-dimensional structure.
[0070] The ICP determination of the removal of different metal ions from the test samples was performed as follows:
[0071] Prepare 150 mg / L of metal salt: weigh Hg(NO3)2 and Pb(NO3)2 respectively and add them into a 100 mL volumetric flask, make up to volume with 0.01 mol / L, pH=7.4 HEPES buffer solution, and perform ultrasonic vibration evenly to completely dissolve the metal salt to obtain a metal cation stock solution with a concentration of 150 mg / L.
[0072] 10 mg of the test sample was added to the above 50 mL of metal ion solution, shaken for 24 hours, and filtered using a filter with a pore size of 0.45 μm. The adsorbed filtrate was collected in a centrifuge tube and the ion concentration was analyzed using ICP-AES.
[0073] Recyclability test of materials after adsorption of metal ions:
[0074] The test sample after the heavy metal ions were adsorbed was added into deionized water with a pH value of 3-4, and then 10% thiourea by volume was added and stirred for 3 hours to desorb the heavy metal ions, and then dried to obtain the dried adsorption material. The above adsorption and removal of different metal ions were continued, and the cycle was repeated 5 times. The adsorption rate and resolution rate of Hg(II) of the adsorption material prepared in Example 3 are shown in Table 1.
[0075] Table 1
[0076]
[0077] Since Ni-MOF has a large amount of uncoordinated N, it can adsorb Hg(II) to form Hg-N bonds. Therefore, Ni-MOF material has a good removal effect on Hg(II) and Pb(II), among which Hg(II) can reach more than 95% and Pb(II) can reach more than 75%. According to Table 1, Ni-MOF has good recyclability for heavy metal adsorption.
[0078] The pyrazole organic monomer prepared in Examples 1 and 2 has a Hg(II) removal rate of 40% and a Pb(II) removal rate of 30%, while the comparative MOF material has an adsorption rate of less than 5% for Pb(II) and Hg(II), and the resolution is too low to be measured.
[0079] The Fe-MOF, Zn-MOF, Mn-MOF, and Co-MOF materials prepared in Examples 3 and 4 have no removal effect on Hg(II) and Pb(II).
[0080] Effect Example 2
[0081] Test sample: Ni-MOF material prepared in Example 3.
[0082] The adsorption interference experiment of Ni-MOF prepared in Example 3 was carried out as follows: Hg(II), Pb(II), Cd(II), Cr(II), Co(II), Ni(II), Ca(II), K(I), Na(I) and Mg(II) metal ion solutions were mixed. The above 10 metal ions were mixed, and the concentration of each metal ion was maintained at 120 mg / L. 10 mg Ni-MOF or Fe-MOF was added, shaken for 24 hours, and filtered using a filter with a pore size of 0.45 μm. The adsorbed filtrate was collected in a centrifuge tube and the ion concentration was analyzed using ICP-AES.
[0083] like Figure 7 As shown, Ni-MOF material has selective adsorption for Hg(II) and is not affected by other ions.
[0084] Effect Example 3
[0085] When the initial concentration of Hg(II) was set to 14 points between 4 and 685 mg / L (4.079, 4.206, 15.26, 36.57, 136.8, 240.6, 136.8, 240.6, 340.6, 421.19, 492.76, 537.53, 586.25, 685.15 mg / L), 10 mg Ni-MOF was added respectively, shaken for 24 hours, and filtered using a filter with a pore size of 0.45 μm. The adsorbed filtrate was collected in a centrifuge tube, and the ion concentration was analyzed using ICP-AES to measure the maximum adsorption of Hg(II) by the Ni-MOF prepared in Example 3. Figure 8 It can be seen that the maximum adsorption amount of Ni-MOF was determined to be 948 mg / g through adsorption experiments.
[0086] Effect Example 4
[0087] 50 mg of Ni-MOF or comparative MOF prepared in Example 3 was added to 50 mL of pure water, tap water or lake water containing Hg(II) (150 mg / L), tetracycline TC (18 mg / L), 17α-ethynyl estradiol EE2 (3 mg / L), rhodamine B RhB (18 mg / L) and methylene blue MB (12 mg / L), and the solution was shaken at 25 ° C for 6 hours and then filtered using a 0.45 μm filter. The adsorbed filtrate was collected in a centrifuge tube and the absorbance was measured using UV-visible spectroscopy. The corresponding concentration was calculated according to the corresponding standard curve (EE2 was quantified using liquid chromatography-mass spectrometry, and Hg(II) content was analyzed using ICP-AES).
[0088] The results are as follows Fig. 9 As shown, the Ni-MOF prepared in Example 3 has excellent degradation effects on all pollutants at the same time and is not affected by the more complex environment in actual wastewater, such as extreme conditions such as pH changes, high temperature, and high salinity.
[0089] In contrast, MOF materials cannot effectively remove heavy metal ions and organic pollutants at the same time, and their adsorption of Hg(II) and Pb(II) and degradation of the above organic matter are both less than 20%.
[0090] The Ni-MOF after adsorbing heavy metal ions and organic pollutants is added into deionized water with pH=3-4, and then 10% thiourea by volume is added and stirred for 3 hours to desorb the heavy metal ions and then dried; the dried material is then soaked in ethanol for 30 minutes and then dried to obtain a dried adsorption material. The dried material still has a good removal rate for heavy metals and various organic pollutants, so the Ni-MOF has good recyclability.
[0091] Effect Example 5
[0092] Take out five 50 ml containers, add 50 mL of tetracycline (40 mg / L) aqueous solution to each container, then add only 10 mg of Fe-MOF prepared in Example 3 to one container, only 5 μM H2O2 to one container, only 0.5 μM PMS to one container, 10 mg of Fe-MOF prepared in Example 3 and 5 μM H2O2 to one container, and 10 mg of Fe-MOF prepared in Example 3 and 0.5 μM PMS to one container. Oscillate the five reactions for 30 minutes, sample at preset time intervals, and filter using a filter with a pore size of 0.45 μm. Collect the adsorbed filtrate in a centrifuge tube, and determine the TC content by liquid chromatography. Test method: Chromatographic column: C18 column (Hypersil GOLD), specification 100 mm*2.1 mm, filler particle size 1.9 um, column temperature 27.5 ° C. Gradient elution: flow rate 0.3 mL / min. 0 to 3 minutes, methanol: water (0.1% formic acid) = 5:95; 3 to 8 minutes, methanol: water (0.1% formic acid) = 95:5, 8 to 10 minutes, methanol: water (0.1% formic acid) = 5:95. Ion source: HESI, ion source temperature 300°C, spray voltage 3.5KV. Mass spectrometry mode: high-resolution FTMS mode, resolution 60000, positive ion collection, mass-to-nuclear ratio range 100-500.
[0093] like Fig.10 It can be seen that Fe-MOF can effectively activate H2O2 and PMS to achieve a degradation rate of more than 98% for TC within 10 minutes.
[0094] like Fig.11 It can be seen that Ni-MOF materials can also activate PMS to accelerate the degradation of various organic pollutants. Fig.11 a), after adding PMS, Ni-MOF can remove 100% of various organic pollutants within 100 minutes ( Fig.11 b).
[0095] The Zn-MOF, Mn-MOF, and Co-MOF materials prepared in Examples 3 and 4 can also activate PMS to accelerate the degradation of various organic pollutants, and can remove 100% of various organic pollutants within 100 minutes.
[0096] Recyclability test of materials after tetracycline removal:
[0097] The Fe-MOF or Ni-MOF material after tetracycline removal was added to ethanol and soaked for 30 minutes, and then dried to obtain the dried Fe-MOF material or Ni-MOF material. The above work of removing tetracycline was continued, and the cycle was repeated 5 times. The removal rate of tetracycline by Fe-MOF material is shown in Table 2.
[0098] Table 2
[0099] Cycle times <![CDATA[Fe-MOF+H2O2]]> Fe-MOF+PMS Ni-MOF+PMS 1 98.45% 98.05% 99.38% 2 94.39% 96.45% 98.14% 3 92.49% 93.09% 97.32% 4 89.09% 92.79% 95.01% 5 86.02% 90.92% 93.55%
[0100] According to Table 2, the Fe-MOF material and the Ni-MOF material still have a good removal rate for various organic pollutants after five cycles of activating PMS or H2O2, so the Fe-MOF material and the Ni-MOF material have good recyclability.
[0101] Effect Example 6
[0102] The catalytic degradation of organic pollutants by Fe-MOF or Ni-MOF activated H2O2 or PMS in actual water bodies was investigated. 5 mg of Fe-MOF or Ni-MOF material was added to the aqueous solution of TC (3 mg / L), RhB (3 mg / L), EE2 (3 mg / L) and bisphenol ABPA (3 mg / L) in Dianchi Lake, Kunming, Yunnan. The reaction was shaken for 3 minutes, and samples were taken at preset time intervals and filtered using a filter with a pore size of 0.45 μm. The adsorbed filtrate was collected in a centrifuge tube, and the content of the corresponding pollutants was determined by liquid chromatography.
[0103] according to Fig.12 It can be seen that under the catalysis of H2O2 or PMS, the degradation rate of TC and RhB of Fe-MOF can reach more than 99%, and the degradation rate of EE2 and BPA can reach more than 70%.
[0104] Under the catalysis of H2O2 or PMS, Ni-MOF can degrade TC, RhB, EE2 and BPA with a degradation rate of more than 90%.
[0105] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A pyrazole organic monomer, characterized in that: Its structural formula is 2. The method for preparing a pyrazole organic monomer according to claim 1, characterized in that: The steps include: (1) First, 1,3,6,8-tetrabromopyrene, 1-(2-tetrahydropyranyl)pyrazole-5-boronic acid pinacol ester, tetrabutylammonium bromide and tetrakis(triphenylphosphine)palladium are placed in an alkaline organic solvent A under an inert gas atmosphere and stirred or ultrasonicated; (2) heating under reflux in an inert gas atmosphere, cooling to room temperature, performing rotary evaporation, extraction, and rotary evaporation, adding alcohol and acid A, ultrasonication, and stirring until the acidification reaction is complete to obtain a suspension; (3) The suspension is poured into water to adjust the pH to 7 to obtain a precipitate, which is then washed and dried to obtain a pyrazole organic monomer.
3. The method for preparing a pyrazole organic monomer according to claim 2, characterized in that: The molar ratio of 1,3,6,8-tetrabromopyrene to 1-(2-tetrahydropyranyl)pyrazole-5-boric acid pinacol ester is 1:(4-8); the molar ratio of 1-(2-tetrahydropyranyl)pyrazole-5-boric acid pinacol ester to tetrabutylammonium bromide is (15-30):1; the molar ratio of 1-(2-tetrahydropyranyl)pyrazole-5-boric acid pinacol ester to tetrakis(triphenylphosphine)palladium is (60-120):1; the organic solvent A is toluene or xylene; the alkali in the alkaline organic solvent A is an aqueous solution of potassium carbonate.
4. The method for preparing a pyrazole organic monomer according to claim 2, characterized in that: In the step (2), the alcohol is methanol or ethanol, and the acid A is nitric acid, hydrochloric acid or sulfuric acid; the time of the acidification reaction is 4-8 hours; the extraction liquid used in the extraction is a mixture of a solvent and water, the solvent is dichloromethane and / or dichloroethane, and the volume ratio of the solvent to water is 1: (0.5-1); the temperature of heating reflux is 100-135° C., the time is 24-72 hours, and the heating method is an oil bath or a sand bath.
5. The method for preparing a pyrazole organic monomer according to claim 2, characterized in that: In the step (3), the volume ratio of the suspension to water is 1:(5-10).
6. A three-dimensional MOF material, characterized in that: A Ni-MOF, Zn-MOF, Mn-MOF, Co-MOF or Fe-MOF metal organic framework material prepared by a solvothermal method using the pyrazole organic monomer described in claim 1 as a ligand and nickel salt, zinc salt, manganese salt, cobalt salt or iron salt as a metal salt.
7. The three-dimensional MOF material according to claim 6, characterized in that: When the metal salt is a nickel salt, the method comprises the following steps: dissolving a pyrazole organic monomer in an organic solvent B, then adding methanol, dimethyl sulfoxide, acid B and a nickel salt solution and ultrasonically obtaining a Ni-MOF; When the metal salt is a zinc salt, the method comprises the following steps: dissolving a pyrazole organic monomer in an organic solvent B, then adding methanol, dimethyl sulfoxide, acid C and a zinc salt solution and ultrasonically obtaining a Zn-MOF; When the metal salt is a manganese salt, the method comprises the following steps: dissolving a pyrazole organic monomer in an organic solvent B, then adding methanol, water, acid B and a manganese salt solution and ultrasonically obtaining Mn-MOF; When the metal salt is a cobalt salt, the method comprises the following steps: dissolving a pyrazole organic monomer in an organic solvent B, and then adding methanol, dimethyl sulfoxide, acid C and a cobalt salt solution and ultrasonically obtaining a Co-MOF; When the metal salt is an iron salt, the method comprises the following steps: dissolving the pyrazole organic monomer in an organic solvent, then adding acetonitrile, dimethyl sulfoxide, acid B and an iron salt solution for ultrasonication, and heating the reaction to obtain Fe-MOF.
8. The three-dimensional MOF material according to claim 7, characterized in that: The organic solvent B is dimethyl sulfoxide, N,N-dimethylformamide or N,N-dimethylacetamide; the concentration of the pyrazole organic monomer in the organic solvent B is 5-20 mg / mL; the acid B is glacial acetic acid, and the acid C is 10% sulfuric acid; the organic solvent B is dimethyl sulfoxide, N,N-dimethylformamide or N,N-dimethylacetamide; the concentration of the pyrazole organic monomer in the organic solvent B is 5-20 mg / mL; the acid B is glacial acetic acid, and the acid C is 10% sulfuric acid; the volume ratio of the methanol, dimethyl sulfoxide, acid B and nickel salt solution or zinc salt solution or cobalt salt solution is 10:(5-10):(0.7-1):(0.1-0.2); The volume ratio of methanol, water, acid B and manganese salt solution is 10:(2-4):(0.7-1):(0.1-0.2); The volume ratio of acetonitrile, dimethyl sulfoxide, acid B and iron salt solution is 10:(2-5):(0.7-1):(0.1-0.2); the concentration of nickel salt solution, zinc salt solution, cobalt salt solution, manganese salt solution or iron salt solution is 0.02 g / mL; The heating reaction temperature is 100-140°C, the time is 12-56h, and the heating rate is 10-20°C / hour.
9. Use of the Ni-MOF metal organic framework material as claimed in claim 7 in removing heavy metal ions and / or organic pollutants in water.
10. Use of the three-dimensional MOF material as claimed in claim 6 in activating PMS or H2O2 to remove organic pollutants in water.
Citation Information
Patent Citations
Cobalt metal organic framework material based on tetra(pyrazolyl)pyrene ligand as well as preparation method and application thereof
CN112625069A
Visible-light-responsive metal-doped pyrazole carboxylic acid MOF (Metal Organic Framework) material as well as preparation method and application thereof
CN118307793A