Salt for magnesium metal battery as well as preparation and application of salt
By using cation- and anion-bound magnesium salts in magnesium batteries to coordinate with heteroatom-containing compounds or Lewis acid-base, the orbital energy level of anions is changed, and the problems of low solubility and passivation film of magnesium salts in magnesium batteries are solved, and the problem of low solubility and passivation film of magnesium salts in magnesium batteries is achieved. The stable circulation and performance of magnesium batteries are improved.
Patent Information
- Application Number
- CN202411029356.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-21
- Filing Date
- 2021-10-20
- Publication Date
- 2024-11-15
AI Technical Summary
The existing magnesium metal batteries have difficulty in selecting electrolytes due to the low solubility of magnesium salt and passivation film problems, which hinders the development of magnesium metal batteries, especially in terms of compatibility and cycling performance between the magnesium negative electrode and the positive electrode.
A magnesium salt is used, which is bound by cations and anions, and changes the orbital energy level of the anions through coordination with heteroatom-containing compounds or Lewis acid-base, so as to form a SEI film and positive electrode that conducts magnesium ions on the negative electrode surface of the magnesium battery. The CEI film is formed on the surface, optimizing the deposition and dissolution process of magnesium.
The stable cycle performance of magnesium batteries under low solubility magnesium salt conditions is achieved, the passivation of the magnesium negative electrode and the decomposition of the electrolyte are suppressed, and the overall performance of magnesium metal batteries is improved.
Smart Images

Figure CN118955548A_ABST
Abstract
Description
[0001] This application is a divisional application of the Chinese invention patent application. The original application date is October 20, 2021, the application number is: 202111222553.8, the name of the invention is: A salt used in magnesium metal batteries and its preparation and application, publication number: CN114380855A; the applicant filed a divisional application. Technical Field
[0002] The present invention belongs to the technical field of salts used in magnesium metal batteries, and relates to a salt used in magnesium metal batteries, and its preparation and application. Specifically, a salt containing a heteroatom compound coordinated with an anion or containing a heteroatom compound and anion having Lewis acid-base action is designed, and its preparation method and application in magnesium metal batteries are designed. Background Art
[0003] Magnesium metal batteries have the advantages of high safety, high volume energy density, and environmental friendliness. 6 S 8 The prototype of the positive electrode. However, the magnesium salt used in the current magnesium metal battery will passivate the magnesium negative electrode by forming a passivation film on the surface of the magnesium negative electrode, which makes it very difficult to select a suitable magnesium salt electrolyte. At present, the solubility of the existing magnesium salt is not very high. It is the lack of magnesium salt electrolyte that makes the development of magnesium battery positive electrode very difficult, which seriously hinders the development of magnesium metal batteries.
[0004] Therefore, it is urgent and necessary to develop salts compatible with magnesium anodes. At present, there are two main methods to develop salt electrolytes compatible with magnesium anodes: one method is to develop salts that do not passivate the magnesium anode and can remove the passivation film on the surface of the magnesium anode, such as Grignard reagent magnesium salts, Mg(BH 4 ) 2 , magnesium salts of carbon-boron cluster anions. Among them, Grignard reagent magnesium salts, Mg(BH 4 ) 2 Magnesium salts not only do not passivate the magnesium negative electrode, but also due to the Grignard reagents or Mg(BH 4 ) 2The strong nucleophilicity can also remove impurities on the surface of the magnesium negative electrode and in the electrolyte that can passivate the magnesium negative electrode. However, this type of electrolyte is incompatible with sulfur positive electrodes or oxide positive electrodes. Although the magnesium salt of carbon boron cluster anions does not passivate the magnesium negative electrode, the production cost is relatively high. Invention patent US10224569B2 reports a method for preparing magnesium salt of carbon boron cluster anions. The quaternary ammonium salt of the carbon boron cluster anion is mixed with a magnesium salt, and then the quaternary ammonium salt cations and the introduced magnesium salt anions are removed in a solvent to obtain the magnesium salt of the carbon boron cluster anion. However, this process is complicated, the cost of the carbon boron cluster anions is high, and quaternary ammonium salt cations and chloride ion impurities will be introduced. Another method is to form a solid electrolyte interface film (SEI film) that can conduct magnesium ions on the surface of the magnesium negative electrode. This SEI film has low electronic conductivity and high ionic conductivity, which can allow magnesium ions to pass quickly. However, most of the existing methods for preparing SEI films are non-in-situ methods, which not only increase the production cost, but also need to be carried out under high temperature conditions. These complex non-in-situ processes have slowed down the development of magnesium metal batteries.
[0005] On the other hand, the coordination or Lewis acid-base interaction of the effective components in the high-concentration salt electrolyte, such as the coordination or Lewis acid-base interaction of anions and cations, and the coordination or Lewis acid-base interaction of cations and solvents, can change the orbital energy levels of the coordinated components, making it easier for the anions or solvents in the electrolyte to form a SEI film on the surface of the metal negative electrode, but this strategy is mainly limited to Li batteries with high solubility of lithium salts. For magnesium batteries with low solubility of magnesium salts, this strategy is not applicable, and it is necessary to provide a salt for constructing a magnesium electrode positive electrode interface film (CEI film) or SEI film. So far, there has been no research on constructing a CEI film on the positive electrode of a magnesium battery. Summary of the invention
[0006] The present invention aims to provide a salt for magnesium metal battery and its preparation and application.
[0007] To achieve the above purpose, the present invention adopts the following technical solution:
[0008] A magnesium salt used in a magnesium metal battery, wherein the salt is formed by the combination of cations and anions, as shown in Formula 1,
[0009]
[0010] T is selected from one of Li, Na, K, Mg, Ca, and Ba; X is selected from halogen; wherein the values of m and n are such that T m X n Display the actual price;
[0011] M is the central atom of the anion, selected from B, Al, C, P or As;
[0012] Y is an atom that forms a bond with M and can be the same or different and is selected from halogen, O, S or NR1 ; When Y is halogen, there is no R group;
[0013] p1, p2 are integers of 0-6, and p1 and p2 are not 0 at the same time; the value of p1+p2 makes the anion have a negative valence;
[0014] q is an integer of 1-6, and the value of q makes the whole salt show 0 valence;
[0015] R, R 1 The same or different ones are selected from C 1 -C 20 Alkyl, C 1 -C 20 The halogenated alkyl, C 3 -C 10 Cycloalkyl, C 3 -C 10 substituted halogenated cycloalkyl, benzene which is unsubstituted or substituted by at least one of the following substituents which are the same or different, wherein the following substituents are halogen, C 1 -C 20 Alkyl, C 1 -C 20 Haloalkyl, C 3 -C 10 Cycloalkyl, C 3 -C 10 and, when p1 and p2 are greater than 1, each R in the formula may be the same or different.
[0016] As mentioned above, the M atom needs to have a larger radius to provide a higher number of bonds in order to change the anion orbital energy level to facilitate its reaction on the positive and negative electrode surfaces of the magnesium battery to form a cross-sectional film, which is ultimately beneficial to the deposition / dissolution of magnesium and inhibits the decomposition of the electrolyte.
[0017] The salt is formed by the combination of a cation and an anion of a bidentate ligand, that is, in Formula 1, when p1 is 0, the salt structure is
[0018] In the formula, m is an integer of 1-10, and n is an integer of 0-10;
[0019] The salt is formed by the combination of a cation and an anion of a monodentate ligand, that is, in Formula 1, when p2 is 0, the salt structure is
[0020] In the formula, m is an integer of 1-10, and n is an integer of 0-10.
[0021] When p1 in Formula 1 is 0, the magnesium salt structural formula is In the formula, m is an integer of 1-10, and n is an integer of 0-10;
[0022] When p2 in Formula 1 is 0, the magnesium salt structural formula is In the formula, m is an integer of 1-10, and n is an integer of 0-10.
[0023] The cation T m X n When T is Mg, Ca, or Ba, T m X n Can be selected from T 2+ , [TX] + ,[T 2 X 3 ] + ,[T 3 X 5 ] + ,[T 4 X 7 ] + or [T 4 X 6 ] 2+ One or more of the following; when T is Li, Na, or K, n is 0.
[0024] For example, when T is Mg, T m X n Mg 2+ , [MgX] + , [Mg 2 X 3 ] + , [Mg 3 X 5 ] + , [Mg 4 X 7 ] + or [Mg 4 X 6 ] 2+ .
[0025] When the group connected to the central atom M of the anion is a -Y group, Y is selected from halogen;
[0026] When the group connected to the central atom M of the anion is a RY-group or a -YRY-group, and p1 and p2 are greater than 1, each R in the formula may be the same or different and may be selected from C 1 -C 20 Alkyl, C 1 -C 20 The halogenated alkyl, C 3 -C 10 Cycloalkyl, C 3 -C 10 substituted halogenated cycloalkyl, benzene which is unsubstituted or substituted by at least one of the following substituents which are the same or different, wherein the following substituents are halogen, C1 -C 20 Alkyl, C 1 -C 20 Haloalkyl, C 3 -C 10 Cycloalkyl, C 3 -C 10 and, when p1 and p2 are greater than 1, each R in the formula may be the same or different; Y may be the same or different and is selected from halogen, O, S or NR 1 .
[0027] The salt structure is Formula 2
[0028]
[0029] The substituents in Formula 2 are consistent with the above description, and A is a compound containing a heteroatom that can change the anion orbital energy level of the salt due to coordination with the central atom M.
[0030] The steric hindrance of the above-mentioned A cannot be too large, so as not to hinder the coordination effect between A and M.
[0031] The group with which A and M coordinate is a heteroatom on the heteroatom-containing compound.
[0032] The heteroatom-containing compound (A) is one or more of alkanes or aromatic hydrocarbons containing at least one heteroatom selected from N, O, S, P, F, Br, Cl, and I; and contains at least one heteroatom-containing compound whose steric hindrance is not too large (i.e., the heteroatom-containing compound cannot hinder its coordination with the anion, and more specifically, there is no substituent other than H on the carbon atom adjacent to the heteroatom in the heteroatom compound;
[0033] Furthermore, A is one or more alkanes or aromatic hydrocarbons containing at least one heteroatom of N, O, S, P, and F.
[0034] Specifically, A is one or more alkanes or aromatic hydrocarbons containing at least one heteroatom of O, S, or N.
[0035] More preferably, the molecular weight of the heteroatom-containing compound (A) is in the range of 50-5,000.
[0036] More preferably, the heteroatom-containing compound (A) is
[0037]
[0038] Wherein k and l are positive integers, i.e. 1-20.
[0039] More preferably, the salt anion is
[0040]
[0041] In the above formula, Y 1 , Y 2 , Y 3 , Y 4 , Y 5 , Y 6 (Y 1 -Y 6 can be collectively referred to as Y) which can be the same or different and are selected from halogen, O, S or NR 1 ; R, R 1 , R 1 , R 2 , R 3 , R 4 , R 5 , R 6 The same or different ones are selected from C 1 -C 20 Alkyl, C 1 -C 20 The halogenated alkyl, C 3 -C 10 Cycloalkyl, C 3 -C 10 substituted halogenated cycloalkyl, benzene which is unsubstituted or substituted by at least one of the following substituents which are the same or different, wherein the following substituents are halogen, C 1 -C 20 Alkyl, C 1 -C 20 Haloalkyl, C 3 -C 10 Cycloalkyl, C 3 -C 10 and, when p1 and p2 are greater than 1, each R in the formula may be the same or different; wherein when Y is a halogen, since the halogen has only a negative valence, there is no R group.
[0042] In further preferred embodiments, R, R 1 , R 1 , R 2 , R 3、 , R 4 , R 5 and R 6 The same or different ones are selected from C 2 -C 20 Fluorinated alkyl, C 3 -C 10 substituted cycloalkyl, benzene which is unsubstituted or substituted by at least one of the following substituents which are the same or different, wherein the following substituents are fluorine, chlorine, C 1 -C 10 Alkyl or C 3 -C 10 of a halogenated cycloalkyl group.
[0043] More preferably, the R, R 1 , R 1 , R 2 , R 3、 , R 4 , R 5 and R 6 The same or different ones are selected from C 3 -C 8 substituted fluorinated alkyl, benzene substituted with at least one of the following substituents which may be the same or different, wherein the following substituents are fluorine, chlorine, C 1 -C 5 of a halogenated alkyl group.
[0044] A method for preparing salt used in magnesium metal batteries:
[0045] When T is Mg, Ca, Ba, the salt is prepared as follows:
[0046] T(MH x ) y As a raw material, in the presence of a reaction solvent containing a heteroatom compound, react with a corresponding -YH compound (Y=O, S, NR) by heating or at room temperature to obtain a salt represented by Formula 1 or Formula 2 in which the heteroatom-containing compound coordinates with an anion or the Lewis acid-base effect changes the orbital energy level of the anion;
[0047] Or, with dialkyl T or TH 2 As a raw material, in the presence of a reaction solvent containing a heteroatom compound, react with the corresponding -YH (Y = O, S, NR) compound, and then add MCl x After the reaction, the heteroatom-containing compound shown in Formula 1 or Formula 2 is coordinated with an anion or undergoes Lewis acid-base action to change the orbital energy level of the anion;
[0048] Or, with MF x As a raw material, in the presence of a reaction solvent containing a heteroatom compound, first react with the corresponding -YH (Y = O, S, NR) compound, and then add the reactant TCl z After the reaction, the heteroatom-containing compound shown in Formula 1 or Formula 2 is coordinated with an anion or undergoes Lewis acid-base action to change the orbital energy level of the anion;
[0049] Or, T(MF x ) y As a raw material, in the presence of a reaction solvent containing a heteroatom compound, react with a corresponding -YH compound (Y=O, S, NR) at 20-120° C. to obtain a salt in which the heteroatom compound shown in Formula 1 or Formula 2 coordinates with an anion or undergoes Lewis acid-base action to change the orbital energy level of the anion;
[0050] In the above reaction, x is a natural number from 1 to 5, z is 1 or 2, and y is 1 or 2.
[0051] When T is Li, Na, K, the salt is prepared as follows:
[0052] T(MH x ) y As a raw material, in the presence of a reaction solvent containing a heteroatom compound, react with a corresponding -YH compound (Y=O, S, NR) by heating or at room temperature to obtain a salt represented by Formula 1 or Formula 2 in which the heteroatom-containing compound coordinates with an anion or the Lewis acid-base effect changes the orbital energy level of the anion;
[0053] Or, T(MF x ) y As a raw material, in the presence of a reaction solvent containing a heteroatom compound, react with a corresponding -YH compound (Y=O, S, NR) at 20-120° C. to obtain a salt in which the heteroatom compound shown in Formula 1 or Formula 2 coordinates with an anion or undergoes Lewis acid-base action to change the orbital energy level of the anion;
[0054] The salt in which the orbital energy level can be changed by the coordination between the heteroatom-containing compound and the anion, that is, the orbital energy level of the anion is changed by the coordination between the heteroatom-containing compound and the anion, thus obtaining the salt described in Formula 2;
[0055] The salt is one in which the orbital energy level of the heteroatom-containing compound and the anion can be changed by interaction, that is, the heteroatom-containing compound and the anion change the orbital energy level of the anion through Lewis acid-base interaction, thus obtaining the salt of formula 1.
[0056] During the above preparation process:
[0057] Raw material Mg(MH x ) y or Mg(MF x ) y Where M is one of B, Al, C, P, and As; x, y are positive integers, and the values of x, y make Mg(MH x ) y or Mg(MF x ) y The overall price is 0;
[0058] Raw material MF x The value of x in MF x It has zero valence, and M is one of B, Al, C, P, and As; MCl x The value of x in MCl x It shows 0 valence, and M is one of B, Al, C, P, and As.
[0059] The amount of the reaction solvent containing the heteroatom compound used in each of the above preparation processes is such that the concentration of the anion is 0.1-4 mol / L;
[0060] The above reaction temperature is 20-120 degrees, and the reaction time is 2-20 hours.
[0061] The reaction solvent of the heteroatom-containing compound may be the same as or different from A, that is, when the reaction solvent of the heteroatom-containing compound is the same as A, the salt shown in Formula 2 is prepared; if the reaction solvent of the heteroatom-containing compound is different from A, it means that the coordination ability of the reaction solvent is weak or the steric hindrance is large (that is, the carbon atom adjacent to the heteroatom in the heteroatom compound contains substituents other than H), and the salt shown in Formula 1 is obtained.
[0062] The -YH compound is C 1 -C 12 Halogenated monohydric alcohol, C 1 -C 12 Halogenated diols, C 1 -C 12 Halogenated monoamine, C 1 -C 12 Halogenated diamine, C 1 -C 6 Halogenated monophenols, C 1 -C 6 Halogenated diphenols, C 1 -C 12 Halogenated monothiol, C 1 -C 12 Halogenated dithiols, C 1 -C 6 Halogenated monothiophenol or C 1 -C 6 Halogenated dihydric thiophenols;
[0063] Preferred -YH compounds are:
[0064] C 1 -C 12 Fluorinated monohydric alcohol, C 1 -C 12 Fluorinated diols, C 1 -C 6 Fluorinated monoamine, C 1 -C 6 Fluorinated diamine, C 1 -C 6 Fluorinated monophenols, C 1 -C 6 Fluorinated diphenols, C 1 -C 12 Fluorinated monothiol, C 1 -C 12Fluorinated dithiols, C 1 -C 6 Fluorinated monothiophenol or C 1 -C 6 Fluorinated dihydric thiophenols;
[0065] The amount of the -YH compound added is such that when all the groups forming a bond with M are -Y-, the molar ratio between the -YH group and the central atom M in the raw material or reactant makes the anion at the center of M have a negative valence of 1;
[0066] When the group bonding to M is partially -Y- and partially halogen, the amount of -YH group and halogen in the raw material or reactant also makes the anion centered on M have a negative valence of 1.
[0067] An application of a salt used in a magnesium metal battery, wherein the salt of structural formula 1 and / or 2 is used as an electrolyte in a magnesium metal battery.
[0068] The electrolyte contains one or more salts in the structural formula 1 and / or one or more salts in the structural formula 2.
[0069] When used as a magnesium battery electrolyte, the anions of the salt of structural formula 1 or 2 coordinate with the heteroatom compound in the electrolyte solvent containing the heteroatom compound or react with Lewis acid and base to change the anion orbital energy level, so that the anions form a layer of SEI film containing inorganic substances on the surface of the negative electrode of the magnesium metal battery that conducts magnesium ions and inhibits the decomposition of the electrolyte; at the same time, a CEI film that can inhibit the decomposition of the electrolyte and the dissolution of the positive transition metal is formed on the surface of the positive electrode. Ultimately, it is beneficial to the deposition and dissolution of magnesium, and finally an excellent magnesium metal battery cycle performance is obtained.
[0070] The salt used does not need to be separated from the reaction system to obtain a solid during its preparation, but the solution obtained after the reaction in the reaction system (i.e., the obtained uniform transparent solution) can be directly used as an electrolyte for magnesium batteries, wherein the salt concentration in the reaction solution is 0.1 mol / L-4.0 mol / L; when the coordination effect or Lewis acid-base effect of the reaction solvent containing the heteroatom compound and the anion is not sufficient to change the orbital energy level of the anion, other heteroatom-containing compounds need to be added to assist in changing the orbital energy level of the anion.
[0071] When the salt used is a solid obtained by preparation and separation, it is mixed with an electrolyte solvent containing a heteroatom compound to form an electrolyte, and the salt concentration in the electrolyte is 0.1 mol / L-4.0 mol / L; wherein, the electrolyte solvent containing the heteroatom compound may be the same as or different from A. When the coordination effect or Lewis acid-base effect of the electrolyte solvent containing the heteroatom compound and the anion is not sufficient to change the orbital energy level of the anion, other heteroatom-containing compounds need to be added to assist in changing the orbital energy level of the anion.
[0072] The battery electrolyte of the present invention has no particular restrictions on the positive electrode.
[0073] The sulfur cathode material of the present invention can be one or more of simple substance S, KB / S, CMK-3 / S, CNT / S, and RGO / S; the selenium cathode material of the present invention can be one or more of simple substance Se, KB / Se, CMK-3 / Se, CNT / Se, and RGO / Se; the cathode material of the present invention can also be a sulfur-selenium composite cathode; the cathode of the present invention can also be Mo 6 S 8 、V 2 O 5 positive electrode.
[0074] The salt electrolyte of the present invention has no particular restrictions on the magnesium negative electrode, and magnesium metal, magnesium alloy or other magnesium composite materials can be selected.
[0075] The advantages of the present invention are:
[0076] The salt provided by the present invention has a central atom of an anion selected from the group consisting of B, Al, C, P, and As, and has a large radius of the central atom, and a small steric hindrance of the negative ion bonded thereto, so that the central atom can further coordinate with a heteroatom-containing compound or react with a Lewis acid and base to change its orbital energy level, and is easy to form a layer of SEI film in situ on the surface of the magnesium metal negative electrode that is conductive to magnesium ions, and can perform reversible magnesium deposition / dissolution; thereby inhibiting the passivation of the magnesium negative electrode and the side reaction of the magnesium negative electrode with the electrolyte, and finally obtaining excellent magnesium metal battery performance. At the same time, a CEI film that can inhibit the decomposition of the electrolyte and the dissolution of the positive transition metal is formed on the positive electrode surface.
[0077] The salt obtained by the present invention is used as the electrolyte of magnesium metal battery. The magnesium ion conductive membrane formed in situ on the negative electrode surface enables the electrolyte that originally cannot be used for magnesium metal battery circulation to be used for magnesium metal battery circulation. At the same time, the formation of this SEI film does not depend on the concentration of magnesium salt. Even low-solubility magnesium salt can coordinate with solvent and anion or Lewis acid-base reaction. In addition, the salt can also form a CEI film on the positive electrode surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0078] Figure 1 This is a single crystal picture of the aluminum central anion coordinated with tetrahydrofuran solvent in Example 1 of the present invention.
[0079] Figure 2 This is a single crystal picture of the aluminum central anion coordinated with ethylene glycol dimethyl ether solvent in Example 2 of the present invention.
[0080] Figure 3 This is a Mg / Mg button cell cycle using the electrolyte in Example 1.
[0081] Figure 4 For magnesium flakes and Mg(TFSI) that have been circulated using the electrolyte in Application Example 1 2 Mo in electrolyte 6 S 8 / Mg battery cycling.
[0082] Figure 5 is the coulombic efficiency of the Mg / Cu button cell cycle using the electrolyte in Example 1.
[0083] Figure 6 The Mo electrolyte in Example 16 was used. 6 S 8 Coulombic efficiency and cycle performance of / Mg button cells.
[0084] Figure 7 For Mo used in the electrolyte of Example 32 6 S 8 / Battery long cycle diagram of Mg battery. DETAILED DESCRIPTION
[0085] The present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0086] The present invention uses the method of coordination of salt anions with heteroatom compounds in the electrolyte or Lewis acid-base action to change the orbital energy level of the anions, so that it is easy to form favorable CEI and SEI films on the surface of the positive and negative electrodes. Since this strategy uses heteroatom compounds to coordinate or interact with anions, high salt concentrations are not required, that is, this strategy is still applicable to salts with low solubility. The reason is that the coordination of heteroatom compounds with anions can change the orbital energy level of anions, so that anions can react with metal negative electrodes to replace magnesium cations in situ, allowing them to shuttle between the positive and negative electrodes. For example, a magnesium metal battery can use sodium salts (lithium salts, potassium salts, etc.) to circulate and replace magnesium ions in situ to obtain magnesium salts, and perform normal circulation of magnesium batteries. Among them, when Li, Na, and K salts are used, better performance will be obtained because the positive and negative electrode CEI and SEI films formed with the participation of Li, Na, and K salts are positive monovalent cations, so they will not produce strong electrostatic attraction to hinder the shuttle of cations.
[0087] Example 1
[0088]
[0089] Under nitrogen atmosphere, 0.334 g of perfluoropinacol was placed in a 50 ml round-bottom flask, and 1 ml of tetrahydrofuran solvent was added; 1.0 mmol of dibutyl magnesium heptane solution was dripped dropwise into the above solution, and the reaction was allowed to react overnight at room temperature to obtain a white precipitate. 0.133 g of anhydrous AlCl was added to the above reaction solution. 3 The solution was stirred overnight to become a homogeneous transparent solution. The above reaction solution was spin-dried to obtain a white solid, which is the magnesium salt of the following structure (see Figure 1 ). The magnesium salt can be directly added with tetrahydrofuran solvent to prepare an electrolyte.
[0090] By structural formula and Figure 1 The single crystal image shows that a tetrahydrofuran molecule in the magnesium salt is coordinated to an aluminum-centered anion to obtain a stable structure.
[0091] Example 2
[0092]
[0093] Under nitrogen atmosphere, 0.334 g of perfluoropinacol was placed in a 50 ml round-bottom flask, and 1 ml of ethylene glycol dimethyl ether solvent was added; 1.0 mmol of dibutyl magnesium heptane solution was dripped dropwise into the above solution, and the reaction was allowed to proceed overnight at room temperature to obtain a white precipitate. 0.133 g of anhydrous AlCl 3 The solution was stirred overnight to become a homogeneous transparent solution. The above reaction solution was spin-dried to obtain a white solid, which is the magnesium salt of the following structure (see Figure 2 ). The magnesium salt can be directly added with ethylene glycol dimethyl ether solvent to prepare an electrolyte.
[0094] By structural formula and Figure 2 The single crystal image shows that a molecule of ethylene glycol dimethyl ether in the magnesium salt is coordinated to an anion centered on the aluminum to obtain a stable structure.
[0095] Example 3
[0096]
[0097] Under nitrogen atmosphere, 0.334 g of perfluoropinacol was placed in a 50 ml round-bottom flask and 1 ml of tetrahydrofuran solvent was added; 0.022 g of Mg(AlH 4 ) 2 The reaction mixture was dried to obtain a white solid, which is the magnesium salt with the following structure. The magnesium salt was directly added with tetrahydrofuran solvent to prepare an electrolyte.
[0098] Example 4
[0099]
[0100] Under nitrogen atmosphere, 0.334 g of perfluoropinacol was placed in a 50 ml round-bottom flask, and 1 ml of ethylene glycol dimethyl ether solvent was added; 0.022 g of Mg(AlH 4 ) 2 The reaction mixture was dried to obtain a white solid, which is the magnesium salt with the following structure. The magnesium salt was directly added with ethylene glycol dimethyl ether solvent to prepare an electrolyte.
[0101] Example 5
[0102]
[0103] Under nitrogen atmosphere, 0.668 g of perfluoropinacol was placed in a 50 ml round-bottom flask, and 5 ml of ethylene glycol dimethyl ether solvent was added; 0.052 g of Ca(AlH 4 ) 2 The reaction mixture was dried to obtain a white solid, which is the calcium salt with the following structure. The calcium salt was directly added with ethylene glycol dimethyl ether solvent to prepare an electrolyte.
[0104] Example 6
[0105]
[0106] Under nitrogen atmosphere, take 0.334g perfluoropinacol into a 50ml round-bottom flask and add 1ml ethylene glycol dimethyl ether solvent; slowly add 0.027g NaAlH 4 The reaction mixture was dried to obtain a white solid, which is the sodium salt with the following structure. The sodium salt was directly added with ethylene glycol dimethyl ether solvent to prepare an electrolyte.
[0107] Example 7
[0108]
[0109] Under nitrogen atmosphere, 0.332 g of hexafluoropropylene oxide was dissolved in 5 ml of tetrahydrofuran, and 0.036 g of water was added to the solution to react overnight. 2.0 mmol of dibutyl magnesium heptane solution was added dropwise to the above solution, and the reaction was carried out at room temperature overnight to obtain a white precipitate. 0.266 g of anhydrous AlCl was added to the above reaction solution. 3 The solution was stirred overnight to become a uniform transparent solution. The reaction solution was spin-dried to obtain a white solid, which was the magnesium salt with the following structure. The magnesium salt was directly added with ethylene glycol dimethyl ether solvent to prepare an electrolyte.
[0110] Example 8
[0111]
[0112] Under nitrogen atmosphere, 0.166 g of hexafluoropropylene oxide was dissolved in 1 ml of ethylene glycol dimethyl ether, and 0.018 g of water was added to the solution to react overnight. 1.0 mmol of dibutyl magnesium heptane solution was added dropwise to the above solution, and the reaction was carried out at room temperature overnight to obtain a white precipitate. 0.133 g of anhydrous AlCl 3 The solution was stirred overnight to become a uniform transparent solution. The reaction solution was spin-dried to obtain a white solid, which was the magnesium salt with the following structure. The magnesium salt was directly added with ethylene glycol dimethyl ether solvent to prepare an electrolyte.
[0113] Example 9
[0114]
[0115] Under nitrogen atmosphere, 0.166 g of hexafluoropropylene oxide was dissolved in 1 ml of tetrahydrofuran, and 0.018 g of water was added to the solution to react overnight; 0.022 g of Mg(AlH 4 ) 2 Continue the reaction for 12 hours and use it directly as an electrolyte. The white solid obtained by spin drying is the magnesium salt in the structural formula.
[0116] Example 10
[0117]
[0118] Under nitrogen atmosphere, 0.166 g of hexafluoropropylene oxide was dissolved in 1 ml of ethylene glycol dimethyl ether, and 0.018 g of water was added to the solution to react overnight; 0.022 g of Mg(AlH 4 ) 2 Continue the reaction for 12 hours and use it directly as an electrolyte. The white solid obtained by spin drying is the magnesium salt in the structural formula.
[0119] Embodiment 11
[0120]
[0121] Under nitrogen atmosphere, 0.334 g of perfluoropinacol was placed in a 50 ml round bottom flask, and 1 ml of ethylene glycol dimethyl ether solvent was added; 0.157 g of Mg(PF 6 ) 2 The powder was reacted at 120 degrees overnight and can be directly used as an electrolyte. The solvent was removed by spin drying to obtain a white solid. This is the magnesium salt with the following structure. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the P center.
[0122] Example 12
[0123]
[0124] Under nitrogen atmosphere, 0.334 g of perfluoropinacol was placed in a 50 ml round bottom flask, and 1 ml of ethylene glycol dimethyl ether solvent was added; 0.214 g of Ba(PF 6 ) 2 The powder can be directly used as an electrolyte after reacting at 80 degrees overnight. The white solid can be obtained by spin drying to remove the solvent. This is the barium salt with the following structure. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the P center.
[0125] Embodiment 13
[0126]
[0127] Under nitrogen atmosphere, take 0.334g perfluoropinacol into a 50ml round-bottom flask, add 2ml tetrahydrofuran solvent; add 1.0mmol dibutylmagnesium heptane solution dropwise into the above solution, react at room temperature overnight to obtain a white precipitate. Add 1.0mmol g of anhydrous BCl 3 , stirring overnight, the solution becomes a uniform transparent solution. The above reaction solution is spin-dried to obtain a white solid, which is the magnesium salt with the following structure. The magnesium salt can be directly added with ethylene glycol dimethyl ether solvent to prepare an electrolyte. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the B center.
[0128] Embodiment 14
[0129]
[0130] Under nitrogen atmosphere, take 0.336g hexafluoroisopropanol in a 50ml round-bottom flask, add 1ml tetrahydrofuran solvent; add 1.0mmol dibutylmagnesium heptane solution dropwise to the above solution, react at room temperature overnight to obtain a white precipitate. Add 1.0mmol anhydrous BCl 3 , stirring overnight, the solution becomes a uniform transparent solution. The above reaction solution is spin-dried to obtain a white solid, which is the magnesium salt with the following structure. The magnesium salt can be directly added with tetrahydrofuran solvent to prepare an electrolyte. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the Al center.
[0131] Embodiment 15
[0132]
[0133] Under nitrogen atmosphere, take 0.334g perfluoropinacol into a 50ml round-bottom flask, add 1ml ethylene glycol dimethyl ether solvent; add 1.0mmol dibutyl magnesium heptane solution dropwise into the above solution, react at room temperature overnight to obtain a white precipitate. Add 1.0mmol anhydrous BCl 3 , stirring overnight, the solution becomes a uniform transparent solution. The above reaction solution is spin-dried to obtain a white solid, which is a magnesium salt with the following structure. The magnesium salt is directly added to a mixed solvent of ethylene glycol dimethyl ether and pyridine to prepare an electrolyte. The anion of the magnesium salt interacts with the mixed solvent containing heteroatom compounds to obtain anions with changed orbital energy levels; the heteroatom compounds in the mixed solvent can be mixed in any proportion.
[0134] Example 16
[0135]
[0136] Under nitrogen atmosphere, take 0.336g hexafluoroisopropanol in a 50ml round-bottom flask, add 1ml ethylene glycol dimethyl ether solvent; add 1.0mmol dibutyl magnesium heptane solution dropwise to the above solution, react at room temperature overnight to obtain a white precipitate. Add 1.0mmol anhydrous BCl 3 , stirring overnight, the solution becomes a homogeneous transparent solution. The magnesium salt is directly added with ethylene glycol dimethyl ether solvent to prepare an electrolyte. The above reaction solution is spin-dried to obtain a white solid, which is the magnesium salt with the following structure. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the B center.
[0137] Embodiment 17
[0138]
[0139] Under nitrogen atmosphere, take 0.334g perfluoropinacol into a 50ml round-bottom flask and add 1ml tetrahydrofuran solvent; slowly add 0.027g KBH 4 Powder, react at room temperature overnight to obtain a white precipitate. The above reaction solution is spin-dried to obtain a white solid, which is the potassium salt with the following structure. The potassium salt is directly added to a mixed solvent of ethylene glycol dimethyl ether and N-methylimidazole to prepare an electrolyte. The anion of the potassium salt interacts with the mixed solvent containing heteroatom compounds to obtain anions with changed orbital energy levels; the heteroatom compounds in the mixed solvent can be mixed in any proportion.
[0140] Embodiment 18
[0141]
[0142] Under nitrogen atmosphere, take 2.016g hexafluoroisopropanol into a 50ml round-bottom flask, add 1ml tetrahydrofuran solvent; slowly add 0.314g Mg(PF 6 ) 2 Powder, react at room temperature overnight to obtain a white precipitate. The above reaction solution is spin-dried to obtain a white solid, which is the magnesium salt with the following structure. The magnesium salt can be directly added with ethylene glycol dimethyl ether solvent to prepare an electrolyte. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the P center.
[0143] Embodiment 19
[0144]
[0145] Under nitrogen atmosphere, 0.334 g of perfluoropinacol was placed in a 50 ml round-bottom flask, and 1 ml of ethylene glycol dimethyl ether solvent was added; 0.014 g of Mg(BH 4 ) 2 Powder, react at room temperature overnight to obtain a white precipitate. The above reaction solution is spin-dried to obtain a white solid, which is the magnesium salt with the following structure. The magnesium salt can be directly added with tetrahydrofuran solvent to prepare an electrolyte. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the B center.
[0146] Embodiment 20
[0147]
[0148] Under nitrogen atmosphere, take 2.00g perfluoropinacol into a 50ml high pressure sealed flask, add 3ml ethylene glycol dimethyl ether solvent; slowly add 0.464g Mg(AsF 6 ) 2 Powder, react at 80 degrees overnight to obtain a white precipitate. The above reaction solution is spin-dried to obtain a white solid, which is the magnesium salt with the following structure. The magnesium salt can be directly added with ethylene glycol dimethyl ether solvent to prepare an electrolyte. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the As center.
[0149] Embodiment 21
[0150]
[0151] Under nitrogen atmosphere, take 0.334g perfluoropinacol into a 50ml round-bottom flask and add 1ml tetrahydrofuran solvent; slowly add 0.142g BF 3 Ether solution was reacted at room temperature overnight to obtain a white precipitate. Then 0.188 g of MgCl2 , heating at 80°C for 12 hours. The reaction solution was dried to obtain a white solid, which is the magnesium salt with the following structure. The magnesium salt can be directly added with ethylene glycol dimethyl ether solvent to prepare an electrolyte. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the B center.
[0152] Embodiment 22
[0153]
[0154] Under nitrogen atmosphere, take 0.334g perfluoropinacol into a 50ml round-bottom flask and add 1ml ethylene glycol dimethyl ether solvent; slowly add 0.142g BF 3 Ether solution was reacted at room temperature overnight to obtain a white precipitate. Then 0.188 g of MgCl 2 , heating at 80°C for 12 hours. The reaction solution was dried to obtain a white solid, which is the magnesium salt with the following structure. The magnesium salt can be directly added with ethylene glycol dimethyl ether solvent to prepare an electrolyte. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the B center.
[0155] Embodiment 23
[0156]
[0157] In a 100 ml round-bottom flask, add 50 ml of diethylene glycol dimethyl ether (G2) solvent, and then add 3.8 g (0.1 mol) of LiAlH 4 , 66.8 g (0.2 mol) of perfluoropinacol was slowly added under ice bath conditions and stirred vigorously. The ice bath was then removed and the reaction was carried out at room temperature for 2 hours, and then refluxed for 6 hours. Then 150 ml of n-hexane was added to precipitate the reaction, and a white solid was obtained, which was the lithium salt of the following structure.
[0158] Embodiment 24
[0159]
[0160] In a 100 ml round-bottom flask, add 50 ml of tetrahydrofuran solvent, then add 3.8 g (0.1 mol) of LiAlH 4 , slowly add 67.2g (0.4mol) of hexafluoroisopropanol under ice bath conditions and stir vigorously. Then remove the ice bath, react at room temperature for 2 hours, and then reflux for 2 hours. Then add 200ml of n-hexane to precipitate it, and obtain a white solid, which is the lithium salt with the following structure.
[0161] Embodiment 25
[0162]
[0163] In a 100 ml round-bottom flask, add 50 ml of tetrahydrofuran solvent, then add 0.1 mol of NaAlH 4 , slowly add 0.1 mol perfluoropinacol under ice bath conditions, stir vigorously, and then add 0.2 mol hexafluoroisopropanol. Then remove the ice bath, react at room temperature for 2 hours, and then reflux for 2 hours. Then add 200 ml of n-hexane to precipitate it, and obtain a white solid, which is the sodium salt with the following structure.
[0164] Embodiment 26
[0165]
[0166] In a 100 ml round-bottom flask, add 50 ml of tetrahydrofuran solvent, then add 0.1 mol of KAlH 4 , slowly add 0.4 mol of pentafluorophenol under ice bath conditions and stir vigorously. Then remove the ice bath, react at room temperature for 2 hours, and then reflux for 2 hours. Then add 200 ml of n-hexane to precipitate it, and obtain a white solid, which is the potassium salt with the following structure.
[0167] Embodiment 27
[0168]
[0169] In a 100 ml round-bottom flask, add 50 ml of tetrahydrofuran solvent, then add 0.1 mol of LiPF 6 , slowly add 0.6 mol of pentafluorophenol under ice bath conditions and stir vigorously. Then remove the ice bath, react at room temperature for 2 hours, and then reflux for 2 hours. Then add 100 ml of toluene to precipitate it, and a white solid is obtained, which is the lithium salt of the following structure. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the P center.
[0170] Embodiment 28
[0171]
[0172] In a 100 ml round-bottom flask, add 50 ml of tetrahydrofuran solvent and then add 0.1 mol of LiAsF 6 , slowly add 0.2 mol perfluoropinacol at room temperature, then add 0.2 mol hexafluoroisopropanol, and stir. Reflux reaction for 12 hours. Then add 100 ml of n-hexane to precipitate it, and a white solid is obtained, which is the lithium salt with the following structure. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the As center.
[0173] Embodiment 29
[0174]
[0175] In a 100ml round-bottom flask, add 50ml of tetrahydrofuran solvent, then add 0.1mol of 2-trifluoromethyl-1,1,1,3,3,3-hexafluoropropane, slowly add 0.1mol of butyl lithium under ice bath conditions, and stir vigorously. Then remove the ice bath, react at room temperature for 2 hours, and reflux for 2 hours. Then add 200ml of n-hexane to precipitate it, and the white solid is the lithium salt with the following structure. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the carbon center.
[0176] Embodiment 30
[0177]
[0178] In a 100 ml round-bottom flask, add 50 ml of tetrahydrofuran solvent, and then add 0.1 mol of LiBH 4 , slowly add 0.1 mol perfluoropinacol under ice bath conditions, stir vigorously, and then add 0.2 mol hexafluoroisopropanol. Then remove the ice bath, react at room temperature for 2 hours, and then reflux for 2 hours. Then add 200 ml of n-hexane to precipitate it, and a white solid is obtained, which is the lithium salt of the following structure. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the B center.
[0179] Embodiment 31
[0180]
[0181] In a 100 ml round-bottom flask, add 50 ml of tetrahydrofuran solvent, then add 0.1 mol of KBH 4 , slowly add 0.1 mol perfluoropinacol under ice bath conditions, stir vigorously, and then add 0.2 mol perfluorotert-butyl alcohol. Then remove the ice bath, react at room temperature for 2 hours, and then reflux for 2 hours. Then add 200 ml of n-hexane to precipitate it, and a white solid is obtained, which is the potassium salt with the following structure. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the B center.
[0182] Embodiment 32
[0183]
[0184] In a 100 ml round-bottom flask, add 50 ml of tetrahydrofuran solvent, then add 0.1 mol of NaPF 6, slowly add 0.2 mol perfluoropinacol under ice bath conditions, then add 0.2 mol hexafluoroisopropanol, and stir vigorously. Then remove the ice bath, react at room temperature for 2 hours, and then reflux for 2 hours. Then add 200 ml of n-hexane to precipitate it, and a white solid is obtained, which is the sodium salt of the following structure. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the P center.
[0185] Embodiment 33
[0186]
[0187] In a 100 ml round-bottom flask, add 50 ml of ethylene glycol dimethyl ether solvent, then add 3.8 g (0.1 mol) of LiAlH 4 , slowly add 49.8g (0.2mol) of tetrachlorocatechol at room temperature and stir. React at room temperature for 2 hours, and then reflux for 4 hours. Then add 120ml of n-hexane to precipitate it, and the white solid is the lithium salt of the following structure. In this structure, although the solvent is not coordinated, the quantitative calculation results show that the solvent will have a strong interaction with the Al center.
[0188] The salt obtained by the above embodiments and a heteroatom compound electrolyte solvent (one or more of the heteroatom-containing compounds that can be used as electrolytes as described above) can be mixed to form a magnesium battery electrolyte; or, the reaction solution obtained by the reaction according to the preparation method of the above embodiment before drying or sedimentation can be directly used as an electrolyte.
[0189] Application Example 1
[0190] Take 150 μL of the 0.5 mol / L reaction solution of magnesium salt prepared in Example 1 (i.e., the uniform transparent solution obtained, and the reaction solution contains tetrahydrofuran with heteroatoms, which can react with anions to change the orbital energy level of anions) and use it as an electrolyte to assemble a 2032-type Mg / Mg symmetrical button battery with a glass fiber diaphragm. The assembled battery is used for performance testing; it can be used at 1.0 mA / cm 2 The current density can be cycled stably for 1000 hours without short circuit (see Figure 3 ). It can be seen that the magnesium salt reaction solution of Example 1 (i.e., the uniform transparent solution obtained) can be used as an electrolyte to perform a stable cycle of a magnesium metal battery.
[0191] Application Example 2
[0192] The recycled magnesium sheet in Application Example 1 was removed from the battery and used as the assembly material for Mo 6 S 8The battery with magnesium metal as the positive electrode and magnesium metal as the negative electrode can obtain stable cycle performance under the conditions of charge cut-off voltage 2.0V and discharge cut-off voltage 0.2V; at the same time, the electrolyte is commercial Mg(TFSI) 2 Soluble in ethylene glycol dimethyl ether, the diaphragm is glass fiber diaphragm, assembled Mo 6 S 8 The negative electrode was replaced with a magnesium sheet that had not been cycled (i.e., ordinary magnesium sheet) as a control; the cycle performance test was carried out under exactly the same conditions as above, and the battery performance of the control group was very poor (see Figure 4 ).Depend on Figure 4 It can be seen that the magnesium salt reaction solution of Example 1 (i.e., the obtained uniform transparent solution) can be used as an electrolyte in a magnesium battery to form a good Mg ion conductive film on the surface of the magnesium negative electrode, and further reversible deposition / dissolution of Mg can be performed.
[0193] Application Example 3
[0194] The 0.5 mol / L reaction solution of magnesium salt prepared in Example 1 (i.e., the obtained uniform transparent solution) was used as an electrolyte, and Cu was directly used as the positive electrode. Then, magnesium metal was used as the negative electrode to assemble a 2032-type button battery. Under the conditions of a charge cut-off voltage of 1.0 V and a discharge cut-off capacity of 0.5 mAh, a stable cycle performance was obtained, and the coulomb efficiency could reach more than 99% (see Figure 5 ).
[0195] Application Example 4
[0196] The 0.5 mol / L reaction solution of magnesium salt prepared in Example 16 was directly used as the electrolyte for Mo 6 S 8 2032 button cell with magnesium metal as the positive electrode and magnesium metal as the negative electrode. Under the conditions of charge cut-off voltage of 2.0V and discharge cut-off voltage of 0.2V, it can obtain stable cycle performance and coulomb efficiency of more than 99% (see Figure 6 ).
[0197] Application Example 5
[0198] The solid lithium salt obtained in Example 23 was prepared into an electrolyte in a glove box with tetrahydrofuran solvent, and the final concentration of lithium salt in the system was 0.5 mol / L, which was then used to assemble a magnesium-sulfur battery. The negative electrode of the magnesium-sulfur battery is a magnesium sheet; the positive electrode of the magnesium-sulfur battery is a mixture of elemental sulfur, conductive carbon black, and a binder in a mass ratio of 6:3:1, and then scraped onto a copper foil with a scraper and dried in a vacuum oven at 60 degrees. The mass of the active material is 0.8 mg / cm2. The magnesium-sulfur battery was assembled with the above positive and negative electrolytes. After 100 cycles at a rate of 0.1C, the capacity retention rate was still 800 mAh / g.
[0199] Application Example 6
[0200] The solid lithium salt obtained in Example 30 was prepared into an electrolyte in a glove box with ethylene glycol dimethyl ether solvent, and the final concentration of lithium salt in the system was 0.5 mol / L, and then used to assemble a magnesium-selenium battery. The negative electrode of the magnesium-selenium battery is a magnesium sheet; the positive electrode of the magnesium-selenium battery is a mixture of elemental selenium, conductive carbon black, and adhesive in a mass ratio of 6:3:1, and then scraped onto a copper foil with a scraper and dried in a vacuum oven at 60 degrees. The mass of the active material is 0.9 mg / cm 2 The magnesium-selenium battery assembled with the above positive and negative electrolytes has a capacity retention rate of 500 mAh / g after 100 cycles at a rate of 0.1C.
[0201] Application Example 7
[0202] The solid sodium salt obtained in Example 32 was prepared into an electrolyte in a glove box with ethylene glycol dimethyl ether solvent to prepare a final sodium salt concentration of 0.5 mol / L in the system, and then used to assemble Mo 6 S 8 / Mg battery. The negative electrode of the battery is a magnesium sheet; Mo 6 S 8 / Mg battery positive electrode is Mo 6 S 8 , conductive carbon black, and adhesive were mixed in a mass ratio of 8:1:1, and scraped onto aluminum foil with a scraper and dried in a vacuum oven at 60 degrees. The mass of active material was 1.2 mg / cm 2 . Use the above positive and negative electrolytes to assemble Mo 6 S 8 / Mg battery, after 300 cycles at 2C rate, still has a capacity retention rate of 115mAh / g. Figure 7 shown.
[0203] Application Example 8
[0204] The solid calcium salt obtained in Example 5 was prepared into an electrolyte in a glove box with a tetrahydrofuran solution, and the final concentration of calcium salt in the system was 0.5 mol / L, and then used to assemble a magnesium-sulfur battery. The negative electrode of the magnesium-sulfur battery is a magnesium sheet; the positive electrode of the magnesium-sulfur battery is a mixture of elemental sulfur, conductive carbon black, and a binder in a mass ratio of 6:3:1, and then scraped onto a copper foil with a scraper and dried in a vacuum oven at 60 degrees. The mass of the active material is 0.8 mg / cm2. The magnesium-sulfur battery was assembled with the above positive and negative electrolytes. After 100 cycles at a rate of 0.1C, the capacity retention rate was still 760 mAh / g.
[0205] Application Example 9
[0206] The solid potassium salt obtained in Example 17 was prepared into an electrolyte in a glove box with ethylene glycol dimethyl ether solvent to prepare a final concentration of potassium salt in the system of 0.5 mol / L, and then used to assemble Mo 6 S 8 / Mg battery. The negative electrode of the battery is a magnesium sheet; Mo 6 S 8 / Mg battery positive electrode is Mo 6 S 8 , conductive carbon black, and adhesive were mixed in a mass ratio of 8:1:1, and scraped onto aluminum foil with a scraper and dried in a vacuum oven at 60 degrees. The mass of active material was 1.2 mg / cm 2 . Use the above positive and negative electrolytes to assemble Mo 6 S 8 / Mg battery, after 500 cycles at a rate of 2C, still has a capacity retention rate of 108mAh / g. XPS, SEM and TEM characterization revealed that the potassium salt can form a SEI film rich in K elements and inorganic substances on the negative electrode surface, and a CEI film rich in inorganic fluorides on the positive electrode surface.
[0207] As can be seen from the above, the central atom of the anion of the salt of structural formula 1 or 2 of the present invention is one of B, Al, C, P or As, and the radius of the central atom is large, and the steric hindrance of the negative ion bonded to it is small, so that the central atom can further coordinate with the heteroatom compound or react with Lewis acid and base to change its orbital energy level, and it is easy to form a layer of inorganic magnesium ion-conducting SEI film on the surface of magnesium metal in situ (that is, there is no need to first construct the SEI film of the magnesium negative electrode and then assemble the magnesium battery), which can perform reversible magnesium deposition / dissolution, thereby inhibiting the passivation of the magnesium negative electrode and the side reaction of the magnesium negative electrode with the electrolyte. At the same time, the anion of the salt can form a CEI film rich in inorganics on the surface of the positive electrode to inhibit the dissolution of transition metals and the decomposition of the electrolyte. Finally, excellent magnesium metal battery performance is obtained.
Claims
1. A salt for use in a magnesium metal battery, characterized in that: Salt is formed by the combination of cations and anions, as shown in Formula 1. T is selected from one of Li, Na, K, Mg, Ca, and Ba; the X group is selected from halogen; wherein the values of m and n are such that T m X n Display the actual price; M is the central atom of the anion, selected from B, Al, C, P or As; Y is an atom that forms a bond with M and may be the same or different and selected from halogen, O, S or NR1; when Y is halogen, there is no R group; p1, p2 are integers of 0-10, and p1 and p2 are not 0 at the same time; the value of p1+p2 makes the anion have a negative valence; q is an integer of 1-6, and the value of q makes the whole salt show 0 valence; R, R1 can be the same or different and can be selected from C1-C 20 Alkyl, C1-C 20 haloalkyl, C3-C 10 Cycloalkyl, C3-C 10 substituted halogenated cycloalkyl, benzene which is unsubstituted or substituted by at least one of the following substituents which are the same or different, wherein the following substituents are halogen, C1-C 20 Alkyl, C1-C 20 Halogenated alkyl, C3-C 10 Cycloalkyl, C3-C 10 and, when p1 and p2 are greater than 1, each R in the formula may be the same or different.
2. The salt used in the magnesium metal battery according to claim 1, characterized in that: The salt is formed by the combination of a cation and an anion of a bidentate ligand, that is, in Formula 1, when p1 is 0, the salt structure is In the formula, m is an integer of 1-10, and n is an integer of 0-10; The salt is formed by the combination of a cation and an anion of a monodentate ligand, that is, in Formula 1, when p2 is 0, the salt structure is In the formula, m is an integer of 1-10, and n is an integer of 0-10.
3. The salt used in the magnesium metal battery according to claim 2, characterized in that: The salt is formed by the combination of a cation and an anion of a bidentate ligand. When T is Mg, the salt structure is: In the formula, m is an integer of 1-10, and n is an integer of 0-10; The salt is formed by the combination of a cation and an anion of a monodentate ligand. When T is Mg, the salt structure is: In the formula, m is an integer of 1-10, and n is an integer of 0-10.
4. The salt used in magnesium metal batteries according to claim 1 or 2, characterized in that: The cation T m X n When T is Mg, Ca, or Ba, T m X n Can be selected from T 2+ , [TX] + , [T2X3] + , [T3X5] + , [T4X7] + or [T4X6] 2+ One or more of the following; when T is Li, Na, or K, n is 0.
5. The salt used in magnesium metal batteries according to claim 1 or 2, characterized in that: When the group connected to the central atom M of the anion in the salt is a -Y group, Y is selected from halogens; When the group connected to the central atom M of the anion is a RY-group or a -YRY-group, and p1 and p2 are greater than 1, each R in the formula may be the same or different and may be selected from C1-C 20 Alkyl, C1-C 20 haloalkyl, C3-C 10 Cycloalkyl, C3-C 10 substituted halogenated cycloalkyl, benzene which is unsubstituted or substituted by at least one of the following substituents which are the same or different, wherein the following substituents are halogen, C1-C 20 Alkyl, C1-C 20 Halogenated alkyl, C3-C 10 Cycloalkyl, C3-C 10 and, when p1 and p2 are greater than 1, each R in the formula may be the same or different; Y may be the same or different and is selected from halogen, O, S or NR1.
6. A method for preparing the salt used in the magnesium metal battery according to claim 1, characterized in that: T(MH x ) y As a raw material, in a reaction solvent containing a heteroatom compound, react with a corresponding -YH compound (Y = O, S, NR) by heating or at room temperature to obtain a salt shown in formula 1; Or, using dialkyl T or TH2 as raw material, reacting with the corresponding -YH (Y=O, S, NR) containing compound in the reaction solvent containing heteroatom compound, and then adding MCl x After the reaction, the salt shown in formula 1 is obtained; Or, with MF x As a raw material, in a reaction solvent containing a heteroatom compound, first react with the corresponding -YH (Y = O, S, NR) compound, and then add the reactant TCl z After the reaction, the salt shown in formula 1 is obtained; Or, T(MF x ) y As a raw material, in a reaction solvent containing a heteroatom compound, react with a corresponding -YH compound (Y=O, S, NR) at 20-120° C. to obtain a salt shown in formula 1; In the above reaction, x is a natural number from 1 to 5, z is 1 or 2, and y is 1 or 2.
7. An application of the salt used in magnesium metal batteries according to claim 1, characterized in that: The salt of structural formula 1 is used as an electrolyte in a magnesium metal battery.
8. An electrolyte for a magnesium metal battery, characterized in that: The electrolyte contains the salt of structural formula 1.
9. The electrolyte of the magnesium metal battery according to claim 8, characterized in that: When the magnesium salt is used in the electrolyte of a magnesium battery, the anions of the salt of structural formula 1 coordinate with the heteroatom compound in the electrolyte or react with Lewis acid and base to change the orbital energy level of the anions, so that the anions form an inorganic interface film on the surface of the positive and negative electrodes of the magnesium battery.
Citation Information
Patent Citations
Method for synthesis of boron cluster based electrolytes for rechargeable magnesium battery
US10224569B2