Preparation method of metal chelate polymer antibody label carrier material with high polymerization degree

Synthesis of high polymerization metal chelated polymer antibody tag carriers through RAFT emulsion polymerization has solved the problems of low sensitivity and few detection channels in the prior art, and achieved efficient labeling detection of low abundance proteins and new metal elements , broaden the number of high-dimensional detection channels for single-cell proteins.

CN118955773AActive Publication Date: 2024-11-15ZHEJIANG UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411040257.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The existing mass spectrometry flow cytometry technology has low sensitivity, few multi-dimensional detection channels, making it difficult to effectively label and detect proteins with low abundance expression, and the loading of new metal elements is insufficient, which limits the expansion of detection channels.

Method used

The RAFT emulsion polymerization method is used to synthesize high-polymerization metal chelated polymer antibody tag carriers, which improves polymerization degree and metal load through chemical modification, enhances signal strength and sensitivity, and introduces a new chelating agent with low insertion rate to broaden the metal isotope channels. quantity.

Benefits of technology

It significantly improves the metal load and detection sensitivity, broadens the number of metal isotope detection channels, can effectively label low-expressed proteins and new metal elements, and improves the ability of high-dimensional detection of single-cell proteins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955773A_ABST
    Figure CN118955773A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-polymerization-degree metal chelate polymer antibody tag carrier material, which comprises the following steps of: preparing a high-polymerization-degree polymer main chain by using an amphiphilic macromolecular reversible addition chain scission chain transfer reagent in combination with an emulsion polymerization method; and functionalizing an end group and a side group through a chemical modification strategy, and grafting a chelating group. A polymer main chain which is high in polymerization degree, narrow in molecular weight distribution and high in terminal group fidelity is creatively prepared through an RAFT emulsion polymerization method, more metal chelating units can be introduced as a tag carrier, more metal atoms can be loaded, the detection signal strength of a labeled antibody can be improved, and the detection sensitivity of the labeled antibody can be improved. And the polymer carrier can be grafted with some novel chelating agents with relatively low efficiency, can load more types of metal isotopes, provides metal detection signals with high sensitivity and more available metal isotope channels in mass spectrum flow detection, and has important significance for realizing single-cell protein analysis and detection with higher precision and higher flux.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of biomedical detection technology, and in particular to a high-polymerization metal chelate polymer antibody label carrier material and a preparation method thereof for labeling antibodies using single-cell protein detection technology based on mass spectrometry flow cytometry. Background Art

[0002] In recent years, time-of-flight mass cytometry (CyTOF), which has high-dimensional detection capabilities and can simultaneously detect protein parameters of more than 50 channels for millions of single cells, has become the most powerful technology for large-scale cell analysis and biomarker discovery. CyTOF uses rare heavy metal isotopes that are not usually present in biological samples to label antibodies and specifically bind to proteins on cells, and then uses a mass spectrometer to detect the time of flight (TOF) of each metal isotope to "read" these isotopes. The TOF of each atom is determined by its mass-to-charge ratio, and the signal intensity is proportional to the number of atoms. Therefore, the composition and content of metal atoms on each cell can be determined by the signal intensity of the corresponding TOF, and then the type and quantity of proteins in a single cell can be associated. At present, high-throughput quantitative analysis of genes and proteins at the single-cell level through CyTOF has become an important technical means for the precise diagnosis and treatment of hematology, oncology and immunology research and related major diseases.

[0003] However, the current mass spectrometry technology still has the problems of low sensitivity and small number of multi-dimensional detection channels. On the one hand, because the number of metal atoms loaded by the existing commercial single polymer antibody label carrier is small (less than 100), and the detection sensitivity of CyTOF is positively correlated with the number of metals, it means that the existing metal labels can only have a good detection effect on cells expressing proteins with high abundance, and there are still sensitivity limitations for the labeling detection of proteins expressed in low abundance. On the other hand, the insertion efficiency of most effective chelators of metal elements on polymers is low, resulting in the current commercial polymer antibody labels can only load specific metal elements through chelators with high insertion rates, including lanthanide, In, Y, Bi, etc., a total of more than 50 metal isotopes, which limits the number of CyTOF detection channels to more than 50. Most of the metal isotope channels have not yet been applied. Therefore, CyTOF is difficult to cover more target proteins in the face of certain complex detection systems, limiting the application and development of multi-channel high-dimensional labeling detection of single-cell proteins.

[0004] However, improving the signal sensitivity of existing polymer antibody labels and expanding the available metal isotope channels is a difficult problem to solve. One of the main reasons is that the existing polymer metal antibody label carrier synthesis process relies on RAFT solution polymerization to synthesize polymer carriers with a narrow molecular weight distribution. In order to ensure the high retention rate of the functional chain ends of the polymerization products, the product polymerization degree is usually low, which limits the number of metal chelating units and makes it difficult to achieve a higher metal loading. For new metal elements, due to the low insertion rate of their effective chelating units on the polymer, the loading amount of new metals on the polymer is even lower, and even the normal labeling sensitivity of the high-expression protein system cannot be achieved. Therefore, it is difficult to further break through the current number of metal isotope channels. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a high-polymerization metal chelate polymer antibody label carrier material for mass spectrometry flow cytometry technology, which greatly increases the metal loading capacity and detection sensitivity compared with existing commercial metal antibody labels, and greatly broadens the number of metal isotope detection channels.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is to provide a method for preparing a metal chelating polymer antibody label carrier material with a high degree of polymerization:

[0007] (1) Synthetic polymer backbone:

[0008] 20 to 80 parts by weight of water, 0.01 to 1.5 parts by weight of an amphiphilic macromolecular reversible addition chain-breaking chain transfer agent, and 1 to 100 parts by weight of a functional monomer are added to a reactor, stirred and mixed, nitrogen is passed through until the air is completely replaced, the temperature is raised to 40 to 80° C., 0.002 to 0.04 parts by weight of a water-soluble initiator is added, and polymerization is initiated for 10 to 60 minutes. An aqueous solution containing 0.01 to 2 parts by weight of an alkali is added, and after the polymerization is completed for 0.5 to 8 hours, the obtained emulsion is demulsified, washed, and dried to obtain a polymer backbone, i.e., an intermediate product A.

[0009] The intermediate product A has the structural formula:

[0010]

[0011] (2) End group functionalization: 1 to 10 parts by weight of the intermediate product A, 1 to 200 parts by weight of a solvent, and 0.05 to 5 parts by weight of a first functionalization reagent are added to a reactor, and the mixture is stirred at room temperature for 2 to 12 hours. After the reaction is completed, the mixture is washed with a solvent, and then the solvent is removed to obtain an intermediate product B.

[0012] The intermediate product B has the structural formula:

[0013]

[0014] (3) Side group functionalization: ① Add 1 to 10 parts by weight of intermediate product B, 1 to 200 parts by weight of solvent, and 1 to 20 parts by weight of second functionalization reagent to the reactor, and stir and react at room temperature for 2 to 12 hours. ② Wash the product and remove the solvent, then add 1 to 200 parts by weight of solvent and 1 to 20 parts by weight of grafting agent to the reactor, and stir and react at room temperature for 2 to 12 hours. ③ Wash the product and remove the solvent, then add 1 to 200 parts by weight of solvent and 1 to 100 parts by weight of chelating agent, stir and mix at room temperature, wash with solvent after the reaction is completed, and then remove the solvent. The final polymer solution is freeze-dried below -20°C to obtain a metal chelate polymer antibody label carrier.

[0015] The first functionalizing agent is selected from ammonia, ammonium bicarbonate, urea, methylamine, dimethylamine, trimethylamine, ethylamine, ethylenediamine, triethylamine, propylamine, isopropylamine, propylenediamine, tripropylamine, ethanolamine, triethanolamine, aniline, benzylamine, and cyclohexylamine; and the second functionalizing agent is selected from formic acid, acetic acid, trifluoroacetic acid, phenol, 1,3-dimethoxybenzene, hydrochloric acid, sulfuric acid, nitric acid, NaH, and HBr.

[0016] The metal chelate polymer antibody tag carrier structure is:

[0017]

[0018] The general chemical structure formula of the amphiphilic macromolecular reversible addition chain scission chain transfer reagent is:

[0019]

[0020] Wherein, the Z group is selected from: phenyl, benzyl, methyl, ethyl, propyl, isopropyl, butyl and its isomers, pentyl and its isomers, ethoxy, methoxy mercaptan, ethylmercapto, isopropylmercapto, butylmercapto, C 12 The R group is selected from the group consisting of 1-methylbenzyl, 1,1-dimethylbenzyl, isopropanoic acid, 2-diisobutyric acid, 2-isobutyronitrile, cyanopentanoic acid, and 3-benzoic acid. The lipophilic monomer includes styrene, acrylate, and methacrylate, and the hydrophilic monomer is selected from acrylic acid and methacrylic acid. The ratio of n to m is 3 to 7. The molecular weight of the amphiphilic macromolecular reversible addition chain scission chain transfer agent is 1000 to 10000.

[0021] Furthermore, the functional monomer of the main chain of the synthetic polymer is one or more of tert-butyl acrylate and tert-butyl methacrylate in any combination; the degree of polymerization of the functional monomer is >100; and the water-soluble initiator is selected from persulfate and azo.

[0022] The aqueous solution containing 0.01 to 2 parts by weight of an alkali, the alkali being selected from sodium hydroxide, potassium hydroxide, aqueous ammonia, sodium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate; and water being 0.1 to 1 parts by weight.

[0023] Furthermore, the grafting agent is NH 2 -R structure, wherein the terminal group of R is selected from amino, N-hydroxysuccinimide, pentafluorophenol ester, carboxyl, aldehyde, thiol, maleimide, vinyl sulfone, azide, alkynyl, hydroxyl, dihydroxyboryl, chlorosiloxane, and o-diphenol.

[0024] Furthermore, the chelating agent is selected from:

[0025]

[0026] The names of the above chelating agents are: porphyrin, nitrilotriacetic acid, ethylenediaminetetraacetic acid, diethyltriaminepentaacetic acid, 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetracarboxylic acid, 1,4,7-triazacyclononane-1,4,7-triacetic acid, hydrazinonicotinamide, dipyridylamine, dehydrogenated phenylcyclopentene, disalicylic aldehyde diamine, R 1 ~R 12 For other substituents, according to the grafting agent NH 2 The group connected to the -R tail is determined as shown in Table 1:

[0027] Table 1: Reaction combinations of groups connected to grafting agents and chelating agents

[0028]

[0029]

[0030] The solvent is selected from toluene, xylene, acetonitrile, dioxane, tetrahydrofuran, acetone, methyl ethyl ketone, dimethyl sulfoxide, dichloromethane, chloroform, tetrachloroethane, methanol, ethanol, isopropanol, ether and water.

[0031] As a second aspect, the present invention provides a metal chelate polymer antibody label carrier material with a high degree of polymerization prepared by the above preparation method.

[0032] The beneficial effects of the present invention are as follows: the RAFT emulsion polymerization method can break through the limitations of the original polymerization process, synthesize a highly active polymer main chain with a degree of polymerization of 100-1000 and a narrow molecular weight distribution (PDI<1.5), and then prepare a metal chelate polymer antibody tag carrier with a high degree of polymerization through chemical modification. The metal loading capacity of the polymer antibody tag carrier prepared by this method increases exponentially with the increase of the degree of polymerization. The degree of polymerization of the currently commercially available polymer antibody tags is generally 100, so the maximum metal ion loading capacity is only 100, which causes the problem of insufficient signal intensity in the detection of low-expression protein systems; at the same time, for chelating units with low insertion rates, the number of other types of metals that can be loaded by the polymer tag is far less than 100, and sensitive detection cannot be achieved, so that the currently available detection channels are limited to more than 50 metal isotopes such as lanthanides. After the present invention prepares a polymer label carrier with a degree of polymerization of 100-1000 through RAFT emulsion polymerization, the metal chelating unit also increases significantly, and the metal loading amount of a single polymer label can be increased by an order of magnitude. On the one hand, compared with the commercial label signal, the signal intensity and sensitivity are significantly enhanced, which provides convenience for the detection of low-expression protein systems; on the other hand, new chelating agents with lower grafting efficiency can be introduced to ensure that the number of these chelating units is still sufficient, and the number of new types of metal isotopes loaded can achieve a more sensitive signal intensity, thereby greatly increasing the types of metal loadings available for polymer labels and greatly broadening the number of CyTOF channels for high-dimensional detection of single-cell proteins. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of porphyrin structure chelating metal;

[0034] Figure 2 Schematic diagram of chelating metals with nitrilotriacetic acid structure;

[0035] Figure 3 Schematic diagram of ethylenediaminetetraacetic acid structure chelating metal;

[0036] Figure 4 Schematic diagram of metal chelation by diethyltriaminepentaacetic acid structure;

[0037] Figure 5 Schematic diagram of chelated metals of 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetracarboxylic acid structure;

[0038] Figure 6 Schematic diagram of chelated metals with 1,4,7-triazacyclononane-1,4,7-triacetic acid structure

[0039] Figure 7 Schematic diagram of hydrazino nicotinamide structure chelating metal

[0040] Figure 8Schematic diagram of the metal chelation structure of dipyridylamine;

[0041] Fig. 9 Schematic diagram of the metal chelate structure of dehexahydrotriphenylcyclopentene;

[0042] Fig.10 This is a schematic diagram of the chelated metal by disalicylicaldehyde diamine structure;

[0043] Fig.11 After marking and staining 100% positive cells in Examples 1-3 and Comparative Example 1, 171 CyTOF signal intensity bar graph detected by Yb channel;

[0044] Fig.12 After marking and staining 100% positive cells for Examples 4 and 5 and Comparative Examples 2 and 3, 120 Sn and 186 CyTOF signal intensity bar graph detected by W channel;

[0045] Fig.13 The results of CyTOF labeling of Sn-loaded polymer antibody labels on 50%:50% yin and yang mixed cells, where (a) is the commercial polymer antibody label of Comparative Example 2, and (b) is the antibody label with a polymerization degree of 1000 in Example 4;

[0046] Fig.14 The CyTOF labeling detection results of the polymer antibody label loaded with W element on 50%:50% yin and yang mixed cells, where (a) is the commercial polymer antibody label of Comparative Example 3, and (b) is the antibody label with a polymerization degree of 1000 in Example 5. DETAILED DESCRIPTION

[0047] The metal chelate polymer antibody tag provided by the present invention is synthesized by the following steps. The first step is to polymerize the functional monomers by RAFT emulsion polymerization to obtain the polymer main chain, the second step is to convert the RAFT group at the end of the main chain into a functional thiol end group by chemical modification, and the third step is to chemically modify the side groups of the main chain, introduce the chelate unit at the side position by a grafting agent, and obtain the antibody tag carrier. The last step is to load the metal on the tag carrier, and then use the active end group to bond with the group on the antibody through a click reaction, and finally obtain the metal-containing tag connected to the antibody.

[0048] The present invention will be further described below in conjunction with specific embodiments and accompanying drawings:

[0049] Example 1

[0050] Synthesize the main chain: 40g of water, 0.8g of amphiphilic macromolecular reversible addition chain scission chain transfer reagent C 12 H 25SS=CS-PS 3 -b-PAA 20 -CH 3 COOH, 5g of tert-butyl methacrylate was added to the reactor, stirred and mixed evenly, nitrogen was passed for 30 minutes (until the air was completely replaced), heated to 70°C, and then an aqueous solution containing 20mg of potassium persulfate was added to initiate polymerization. When the reaction lasted for 10 minutes, an aqueous solution containing 0.15g of sodium hydroxide was added, and the polymerization was continued for 2 hours. After the polymerization was completed, hydrochloric acid was added until the emulsion was completely broken, neutralized, washed, filtered, and vacuum dried to obtain the polymer main chain product.

[0051] End group modification: Weigh 1 g of the above polymer solid and add it to the reactor, add 5 mL of acetone and stir to completely dissolve it, then add 0.6 g of benzylamine and stir to react at room temperature for 12 hours. After the reaction is completed, the solvent is removed by rotary evaporation to obtain an end group functionalized product.

[0052] Side group modification: Add 20mL of dichloromethane and 10mL of acetic acid to the above-mentioned terminal functionalized product, stir and react for 12h after mixing, then filter out the solution, add an appropriate amount of dichloromethane to wash the polymer product, and then evaporating to remove the solvent. Then add 10mL of deionized water to dissolve the polymer, then add 5g of mercaptoethylamine, stir and react at room temperature for 12h, then wash with water, and then ultrafilter to remove water. Then add 20mL of water, then add 30g of 1,4,7-triazacyclononane-1,4,7-triacetic acid-2-maleimide, stir and react at room temperature for 1h. After the reaction is completed, add water to wash the product, then ultrafilter to remove water, and finally freeze-dry the polymer aqueous solution below -20 degrees, and then seal it at a low temperature below -20 degrees.

[0053] To prepare the metal antibody tag, take 1 mg of the lyophilized polymer powder prepared by the above method and add 100 μL of 40 mM YbCl 3 Solution (dissolved with PBS buffer at pH = 7.0), react at 37°C for 1 hour; after the reaction, transfer to an ultrafiltration tube, wash, centrifuge, remove the supernatant, add 0.1 mg of antibody, mix well, and react at 37°C for 0.5 hour. After the reaction, transfer to an ultrafiltration tube, centrifuge, remove the supernatant, and obtain the metal tag connected to the antibody.

[0054]

[0055] Example 2

[0056] Synthesize the main chain: 40g of water, 0.16g of amphiphilic macromolecular reversible addition chain scission chain transfer reagent C 12 H 25 SS=CS-PS 5 -b-PAA20 -CH 3 COOH, 5g of tert-butyl acrylate was added to the reactor, stirred and mixed, stirred, nitrogen was passed for 30 minutes, heated to 60°C, and an aqueous solution containing 4mg of azobiscyanovaleric acid was added to initiate polymerization. When the reaction lasted for 20 minutes, an aqueous solution containing 0.045g of sodium hydroxide was added, and the polymerization was continued for 4 hours. After the polymerization was completed, hydrochloric acid was added until the emulsion was completely broken, neutralized, washed, filtered, and vacuum dried to obtain the polymer main chain product.

[0057] End group modification: Weigh 1 g of the above polymer solid and add it to the reactor, add 5 mL of tetrahydrofuran and stir to completely dissolve it, then add 0.3 g of propylamine and stir to react at room temperature for 12 hours. After the reaction is completed, the solvent is removed by rotary evaporation to obtain an end group functionalized product.

[0058] Side group modification: Add 20mL of chloroform and 10mL of formic acid to the above-mentioned terminal functionalized product, stir and react for 12h after mixing, then filter out the solution, add an appropriate amount of chloroform to wash the polymer product, and then remove the solvent by rotary evaporation. Then add 10mL of water to dissolve the polymer, then add 4g of propylenediamine, stir and react at room temperature for 12h, then wash with water, and then ultrafilter to remove water. Then add 20mL of water, then add 50g of diethyltriaminepentaacetic acid, stir and react at room temperature for 1h. After the reaction is completed, add water to wash the product, then ultrafilter to remove water, and finally freeze-dry the polymer aqueous solution below -20 degrees, and then seal it at a low temperature below -20 degrees.

[0059] To prepare the metal antibody tag, take 5 mg of the lyophilized polymer powder prepared by the above method and add 100 μL of 200 mM YbCl 3 Solution (dissolved with PBS buffer at pH = 7.0), react at 37°C for 1 hour; after the reaction, transfer to an ultrafiltration tube, wash, centrifuge, remove the supernatant, add 0.1 mg of antibody, mix well, and react at 37°C for 0.5 hour. After the reaction, transfer to an ultrafiltration tube, centrifuge, remove the supernatant, and obtain the metal tag connected to the antibody.

[0060]

[0061] Example 3

[0062] Synthesize the main chain: 40g of water, 0.08g of amphiphilic macromolecular reversible addition chain scission chain transfer reagent C 12 H 25 SS=CS-PS 6 -b-PAA 17 -CH 3COOH, 5g of tert-butyl methacrylate was added to the reactor, stirred and mixed, stirred, nitrogen was passed for 30 minutes, heated to 50°C, and an aqueous solution containing 2mg of azobisisobutylimidazoline hydrochloride was added to initiate polymerization. When the reaction lasted for 30 minutes, an aqueous solution containing 0.03g of sodium hydroxide was added, and the polymerization was continued for 6 hours. After the polymerization was completed, hydrochloric acid was added until the emulsion was completely broken, neutralized, washed, filtered, and vacuum dried to obtain the polymer main chain product.

[0063] End group modification: Weigh 1 g of the above polymer solid and add it to the reactor, add 5 mL of isopropanol and stir to completely dissolve it, then add 0.5 g of aniline and stir to react at room temperature for 12 hours. After the reaction is completed, the solvent is removed by rotary evaporation to obtain the end group functionalized product.

[0064] Side group modification: Add 20 mL of tetrahydrofuran and 25 g of phenol to the above-mentioned terminal functionalization product, stir and react for 12 hours after mixing, then filter out the solution, add 20 mL of tetrahydrofuran to wash the polymer product, and then evaporating to remove the solvent. Then add 10 mL of water to dissolve the polymer, then add 8 g of alkynylethylamine, stir and react at room temperature for 12 hours, then wash with water, and then ultrafilter to remove water. Then add 20 mL of water, then add 80 g of 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetraacetic acid-2-azido, stir and react at room temperature for 1 hour. After the reaction is completed, add water to wash the product, then ultrafilter to remove water, and finally freeze-dry the polymer aqueous solution below -20 degrees, and then seal it at a low temperature below -20 degrees.

[0065] To prepare the metal antibody tag, 10 mg of the lyophilized polymer powder prepared by the above method was added with 100 μL of 400 mM YbCl 3 Solution (dissolved with PBS buffer at pH = 7.0), react at 37°C for 1 hour; after the reaction, transfer to an ultrafiltration tube, wash, centrifuge, remove the supernatant, add 0.1 mg of antibody, mix well, and react at 37°C for 0.5 hour. After the reaction, transfer to an ultrafiltration tube, centrifuge, remove the supernatant, and obtain the metal tag connected to the antibody.

[0066]

[0067] Example 4

[0068] Synthesize the main chain: 40g of water, 0.08g of amphiphilic macromolecular reversible addition chain scission chain transfer reagent C 12 H 25 SS=CS-PS 6 -b-PAA 17 -CH 3COOH, 5g of tert-butyl acrylate was added to the reactor, stirred and mixed, stirred, nitrogen was passed for 30 minutes, heated to 50°C, and an aqueous solution containing 2mg of azobisisobutylimidazoline hydrochloride was added to initiate polymerization. When the reaction lasted for 30 minutes, an aqueous solution containing 0.03g of sodium hydroxide was added, and the polymerization was continued for 6 hours. After the polymerization was completed, hydrochloric acid was added until the emulsion was completely broken, neutralized, washed, filtered, and vacuum dried to obtain the polymer main chain product.

[0069] End group modification: Weigh 1g of the above polymer solid and add it to the reactor, add 5mL of methanol and stir to completely dissolve it, then add 1g of cyclohexylamine and stir to react at room temperature for 12h. After the reaction is completed, the solvent is removed by rotary evaporation to obtain the end group functionalized product.

[0070] Side group modification: Add 20mL of ether and 10mL of trifluoroacetic acid to the above-mentioned end functionalization product, stir and react for 12h after mixing, then filter out the solution, add 20mL of ether to wash the polymer product, and then remove the solvent by rotary evaporation. Then add 10mL of water to dissolve the polymer, add 6g of ethylenediamine, stir and react at room temperature for 12h, then wash with water, and then ultrafilter to remove water. Finally, add 20mL of water to dissolve, add 120g of tetracarboxylphenylporphyrin, and stir and react at room temperature for 1h. After the reaction is completed, add water to wash the product, then ultrafilter to remove water, and finally freeze-dry the polymer aqueous solution below -20 degrees, and then seal it at a low temperature below -20 degrees.

[0071] To prepare the metal antibody tag, 10 mg of the lyophilized polymer powder prepared by the above method was added with 100 μL of 400 mM SnCl 2 Solution (dissolved with dilute hydrochloric acid solution at pH = 2.0), reacted at 37°C for 1 hour; after the reaction, transferred to an ultrafiltration tube, washed with PBS buffer at pH = 7.0 for multiple times, centrifuged, removed the supernatant, and then added 0.1 mg of antibody and mixed thoroughly, reacted at 37°C for 0.5 hour. After the reaction, transferred to an ultrafiltration tube, centrifuged, removed the supernatant, and obtained the metal tag connected to the antibody.

[0072]

[0073] Example 5

[0074] Synthesize the main chain: 40g of water, 0.08g of amphiphilic macromolecular reversible addition chain scission chain transfer reagent C 12 H 25 SS=CS-PS 6 -b-PAA 17 -CH 3COOH, 5g of tert-butyl acrylate was added to the reactor, stirred and mixed, stirred, nitrogen was passed for 30 minutes, heated to 50°C, and an aqueous solution containing 2mg of azobisisobutylimidazoline hydrochloride was added to initiate polymerization. When the reaction lasted for 30 minutes, an aqueous solution containing 0.03g of sodium hydroxide was added, and the polymerization was continued for 6 hours. After the polymerization was completed, hydrochloric acid was added until the emulsion was completely broken, neutralized, washed, filtered, and vacuum dried to obtain the polymer main chain product.

[0075] End group modification: Weigh 1g of the above polymer solid and add it to the reactor, add 5mL of dichloromethane and stir to completely dissolve it, then add 0.15g of triethylamine and stir to react at room temperature for 12h. After the reaction is completed, the solvent is removed by rotary evaporation to obtain the end group functionalized product.

[0076] Side group modification: Add 20mL of acetone and 10mL of formic acid to the above-mentioned end functionalization product, stir and react for 12h after mixing, then filter out the solution, add 20mL of acetone to wash the polymer product, and then remove the solvent by rotary evaporation. Then add 10mL of water to dissolve the polymer, then add 10g of dihydroxyborylethylamine, stir and react at room temperature for 12h, then wash with water, and then ultrafilter to remove water. Then add 20mL of water to dissolve, then add 100g of dehydrobenzocyclopentene, stir and react at room temperature for 1h. After the reaction is completed, add water to wash the product, then ultrafilter to remove water, and finally freeze-dry the polymer aqueous solution below -20 degrees, and then seal it at a low temperature below -20 degrees.

[0077] Preparation of metal antibody tag: Take 10 mg of the polymer lyophilized powder prepared by the above method, add 100 μL of 400 mM Na 2 WO 4 .2H 2 O aqueous solution, react at 37°C for 1h; after the reaction, transfer to an ultrafiltration tube, wash with pH=7.0 PBS buffer several times, centrifuge, remove the supernatant, add 0.1mg of antibody, mix well, and react at 37°C for 0.5h. After the reaction, transfer to an ultrafiltration tube, centrifuge, remove the supernatant, and obtain the metal tag connected to the antibody.

[0078]

[0079] Comparative Example 1

[0080] Take 1 mg of the commercial polymer antibody tag carrier lyophilized powder of fluidium and add it to the reaction tube, then add 100 μL of 40 mM YbCl 3Solution (dissolved with PBS buffer at pH = 7.0), react at 37°C for 1 hour; after the reaction, transfer to an ultrafiltration tube, wash, centrifuge, remove the supernatant, add 0.1 mg of antibody, mix well, and react at 37°C for 0.5 hour. After the reaction, centrifuge, remove the supernatant, and obtain the metal tag connected to the antibody.

[0081] Comparative Example 2

[0082] Take 1 mg of the commercial polymer antibody tag carrier lyophilized powder of fluidium and add it to the reaction tube, then add 100 μL of 40 mM SnCl 2 Solution (dissolved with dilute hydrochloric acid solution at pH = 2.0), react at 37°C for 1 hour; after the reaction, transfer to an ultrafiltration tube, add PBS buffer at pH = 7.0 for washing, centrifuge, remove the supernatant, add 0.1 mg of antibody, mix well, and react at 37°C for 0.5 hour. After the reaction, centrifuge, remove the supernatant, and obtain the metal tag connected to the antibody.

[0083] Comparative Example 3

[0084] Take 1 mg of the commercial polymer antibody tag carrier lyophilized powder of fluidium and add it to the reaction tube, then add 100 μL of 400 mM Na 2 WO 4 .2H 2 O aqueous solution, react at 37°C for 1 hour; after the reaction is completed, transfer to an ultrafiltration tube, add pH=7.0 PBS buffer for washing, centrifuge, remove the supernatant, add 0.1 mg of antibody, mix well, and react at 37°C for 0.5 hour. After the reaction is completed, centrifuge, remove the supernatant, and obtain the metal tag connected to the antibody.

[0085] The degree of polymerization, molecular weight distribution index and end group retention rate of the polymer backbone of Examples 1-5 are shown in Table 2. The actual number of polymerized units can basically reach the designed degree of polymerization of 100-1000, and maintain a narrow molecular weight distribution with a molecular weight distribution index of <1.5, and the end group activity retention rate>96%.

[0086] Table 2 Degree of polymerization, molecular weight distribution, and end group retention rate of polymer antibody label carriers

[0087] Example Design aggregation Actual number of aggregate units Molecular weight distribution index End group retention rate 1 100 102 1.21 99% 2 500 495 1.31 99% 3 1000 986 1.35 98% 4 1000 977 1.42 97% 5 1000 982 1.43 96%

[0088] The metal ion concentration in the antibody label sample solution was tested by ICP-MS, and the metal loading on a single polymer chain was calculated by the known polymer concentration. The number of chelating agents was characterized by nuclear magnetic resonance, and the results are shown in Table 3. Examples 1-3 show that with the increase of the degree of polymerization, the number of chelating units and the metal loading also doubled, up to nearly 1000; Examples 4 and 5 show that although the insertion rate of chelating agents such as porphyrin and dehydrobenzocyclopentene on the polymer is low, the total number of grafting of the chelating agent on the high-polymerization polymer antibody label carrier prepared by the present invention can reach more than 100, so that the total amount of the new metal elements Sn and W effectively loaded can reach or even exceed the metal quantity of the traditional commercial polymer antibody label; Comparative Examples 1-3 show that the use of commercial polymer antibody labels can only have a high loading efficiency for lanthanide elements such as Yb, while the loading amount for new metal elements such as Sn and W is extremely low.

[0089] Table 3 Metal loading of metal chelating polymer antibody labels

[0090]

[0091] Cell staining test experiment:

[0092] (1) Using the eight antibody label materials of Examples 1-5 and Comparative Examples 1-3, 100% positive cells (expressing antigenic proteins specifically recognized by antibodies) were labeled and stained to characterize the signal intensity.

[0093] (2) Using the antibody label materials of Examples 4 and 5 and Comparative Examples 2 and 3, a mixture of 50% negative cells (not expressing antigen proteins specifically recognized by antibodies) and 50% positive cells was labeled and stained to detect the clustering effect.

[0094] The labelled cell staining method is as follows:

[0095] 1. Prepare several groups of normal living cells, about 2×10^6 cells in each group, resuspend them in PBS buffer, adjust the volume to 1mL, add Rh-103, stain at room temperature for 5 minutes, and distinguish between dead and live cells.

[0096] 2. Add 2 mL of 0.5-5 mg / mL bovine serum albumin solution to each group, centrifuge at 500 x g for 5 min, remove the supernatant, add 50 μL of blocking solution (0.5 μL of 0.5-1.5 mg / mL human immunoglobulin solution, 0.5 μL of 0.5-1.5 mg / mL mouse immunoglobulin solution, 0.5 μL of 0.5-1.5 mg / mL rat immunoglobulin solution, 0.5 μL of 0.5-1.5 mg / mL hamster immunoglobulin solution, 48 μL of 0.5-5 mg / mL bovine serum albumin solution), and block on ice for 20 min.

[0097] 3. Add 50 μL of extracellular antibody mixture (polymer antibody label, the antibody concentration is 0.1-1 mg / mL), resuspend the cells, and stain on ice for 30 minutes.

[0098] 4. Add 2 mL of 0.5-5 mg / mL bovine serum albumin solution, centrifuge at 500 x g for 5 min, remove the supernatant, add 1 mL of fix and perm cell mixture (fluidigm) containing 0.5 v / v‰ single cell indicator 191 / 193Ir (fluidigm), resuspend the cells, and incubate at 4°C overnight.

[0099] 5. Add 2 mL of 0.5-5 mg / mL bovine serum albumin solution, centrifuge at 800 x g for 5 min, remove the supernatant, and repeat twice.

[0100] 6. Add 2 mL of deionized water, centrifuge at 800 x g for 5 min, remove the supernatant, and repeat twice.

[0101] 7. Filter the sample, count the cells, adjust the volume, prepare for mass spectrometry flow cytometry.

[0102] The labeling signal intensity of 100% positive cells in Examples 1-3 and Comparative Example 1 is as follows: Fig.11 It can be found that the signal intensity increases exponentially with the degree of polymerization of the polymer label. The signal intensity of MCP-500 and MCP-1000 increases by nearly 5 times and 10 times respectively compared with the commercial CMCP label, which significantly increases the labeling sensitivity.

[0103] The labeling signal intensity of positive cells in Examples 4-5 and Comparative Examples 2-3 is as follows Fig.12 As shown. In Example 4, Sn 120 The signal intensity of the channel is much higher than that of Comparative Example 2, while that of Example 5 is 186 The signal intensity of the channel is much higher than that of Comparative Example 3, indicating that the chelating agent of the current commercial tags cannot effectively load metals such as Sn and W, resulting in a very low metal signal intensity; while the MCP-1000 prepared by the present invention can greatly increase the number of low insertion rate chelating agents to effectively load enough Sn and W, thereby obtaining a higher detection sensitivity on these metal isotope channels.

[0104] The staining results for 50%:50% mixed Yin and Yang cells are as follows: Figure 13-14 As shown, the horizontal axis 191Ir represents the situation of DNA staining, which proves that it is a cell signal; the ordinate is the corresponding metal isotope signal intensity. It can be found that in the Sn and W channels, the signal intensity of Comparative Examples 2 and 3 is very low, and it is impossible to distinguish between positive and negative cell groups; Examples 4 and 5 can clearly divide the negative and positive groups, and the proportion of the positive group is close to the actual value of 50%, indicating that the sensitivity of the label detection is high, and the target cells can be separated from the non-target cells. Therefore, it is explained that the polymer antibody label prepared by the present invention can be applied to the sensitive labeling detection of new metal elements such as Sn and W by increasing the degree of polymerization and greatly increasing the number of new chelating agents with low insertion rates.

[0105] The above embodiments are only used to illustrate the present invention, but are not used to limit the scope of implementation of the present invention.

Claims

1. A method for preparing a metal chelating polymer antibody tag carrier material with a high degree of polymerization, It is characterized in that The steps include: 20 to 80 parts by weight of water, 0.01 to 1.5 parts by weight of an amphiphilic macromolecular reversible addition chain-breaking chain transfer agent, and 1 to 100 parts by weight of a functional monomer are added to a reactor, stirred and mixed, nitrogen is passed through until the air is completely replaced, the temperature is raised to 40 to 80° C., 0.002 to 0.04 parts by weight of a water-soluble initiator is added, polymerization is carried out for 10 to 60 minutes, an aqueous solution containing 0.01 to 2 parts by weight of an alkali is added, polymerization is carried out for 0.5 to 8 hours, and then the obtained emulsion is demulsified, washed, and dried to obtain an intermediate product A; 1 to 10 parts by weight of intermediate product A, 1 to 200 parts by weight of solvent, and 0.05 to 5 parts by weight of first functionalization reagent are stirred and reacted at room temperature for 2 to 12 hours; washing with a solvent and removing the solvent to obtain an intermediate product B; Add 1 to 10 parts by weight of the intermediate product B, 1 to 200 parts by weight of the solvent, and 1 to 20 parts by weight of the second functionalizing agent to the reactor, stir and react at room temperature for 2 to 12 hours, filter, wash with a solvent, and remove the solvent; add 1 to 200 parts by weight of the solvent and 1 to 20 parts by weight of the grafting agent, stir and react at room temperature for 2 to 12 hours, wash with a solvent, and remove the solvent; add 1 to 200 parts by weight of the solvent and 1 to 100 parts by weight of the chelating agent, stir at room temperature until mixed, wash with a solvent, and remove the solvent; freeze-dry below -20°C to obtain; Among them, the first functionalizing agent is selected from ammonia water, ammonium bicarbonate, urea, methylamine, dimethylamine, trimethylamine, ethylamine, ethylenediamine, triethylamine, propylamine, isopropylamine, propylenediamine, tripropylamine, ethanolamine, triethanolamine, aniline, benzylamine, and cyclohexylamine; and the second functionalizing agent is selected from formic acid, acetic acid, trifluoroacetic acid, phenol, 1,3-dimethoxybenzene, hydrochloric acid, sulfuric acid, nitric acid, NaH, and HBr.

2. The preparation method according to claim 1, It is characterized in that The general chemical structure formula of the amphiphilic macromolecular reversible addition chain scission chain transfer reagent is: wherein the Z group is selected from phenyl, benzyl, methyl, ethyl, propyl, isopropyl, butyl and its isomers, pentyl and its isomers, ethoxy, methoxymercaptan, ethylmercapto, isopropylmercapto, butylmercapto, C 12 The R group is selected from 1-methylbenzyl, 1,1-dimethylbenzyl, isopropanoic acid, 2-diisobutyric acid, 2-isobutyronitrile, cyanopentanoic acid, and 3-benzoic acid; the lipophilic monomer is selected from styrene, acrylate, and methacrylate, and the hydrophilic monomer is selected from acrylic acid and methacrylic acid. The ratio of n to m is 3 to 7.

3. The preparation method according to claim 2, It is characterized in that The molecular weight of the amphiphilic macromolecular reversible addition-fragmentation chain transfer agent is 1,000 to 10,000.

4. The preparation method according to claim 1, It is characterized in that The functional monomer is one or more of tert-butyl acrylate and tert-butyl methacrylate in any proportion, and the degree of polymerization of the functional monomer is greater than 100; The water-soluble initiator is selected from persulfate and azo.

5. The preparation method according to claim 1, It is characterized in that The aqueous solution containing 0.01 to 2 parts by weight of an alkali, wherein the alkali is selected from sodium hydroxide, potassium hydroxide, ammonia water, sodium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate; and water is 0.1 to 1 part by weight.

6. The preparation method according to claim 1, It is characterized in that The grafting agent is NH 2 -R structure, wherein the terminal group of R is selected from amino, N-hydroxysuccinimide, pentafluorophenol ester, carboxyl, aldehyde, thiol, maleimide, vinyl sulfone, azide, alkynyl, hydroxyl, dihydroxyboryl, chlorosiloxane, and o-diphenol.

7. The preparation method according to claim 1, It is characterized in that The chelating agent is selected from: Among them, R 1 ~R 12 Determined according to the terminal group of the grafting agent NH2-R, as shown in the following table:

8. The preparation method according to claim 1, It is characterized in that The solvent is selected from toluene, xylene, acetonitrile, dioxane, tetrahydrofuran, acetone, methyl ethyl ketone, dimethyl sulfoxide, dichloromethane, chloroform, tetrachloroethane, methanol, ethanol, isopropanol, ether and water.

9. A metal chelating polymer antibody label carrier material with a high degree of polymerization prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method for preparing reversible addition-fragmentation chain transfer emulsion polymerization

    CN101591403A

  • Method for preparing high molecular weight and segmented polymers by reversible addition-fragmentation chain transfer emulsion polymerization

    CN101591405A

  • Metal-marked polymeric microbeads with

    CN117203278A

  • Polymeric metal chelating compositions and methods of preparing same for controlling growth and activities of living cells and organisms

    US20190169126A1

  • Reagents and methods for elemental mass spectrometry of biological samples

    US20210239707A1