Antibacterial and deodorant super absorbent resin material and preparation method thereof

By grafting cationic or zwitterionic ions onto superabsorbent resin and adding deodorizing components, the problems of poor antibacterial durability and complex preparation of existing superabsorbent resins are solved, achieving long-lasting antibacterial and deodorizing effects and improved water absorption, making it suitable for disposable hygiene products.

CN118955780AActive Publication Date: 2024-11-15SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
CN202410923462.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-15
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

Existing antibacterial and deodorizing superabsorbent resins suffer from problems such as complex manufacturing processes, poor antibacterial durability, and poor biocompatibility of inorganic antibacterial agents.

Method used

By grafting cationic or zwitterionic ions onto the three-dimensional structure of superabsorbent resin through addition polymerization and adding deodorizing components, a superabsorbent resin with long-lasting antibacterial and deodorizing functions can be prepared.

Benefits of technology

It achieves long-lasting antibacterial and deodorizing properties of superabsorbent resin, improves the water absorption of the material, and has a simple preparation process, making the antibacterial substances difficult to dissolve and safe and non-toxic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955780A_ABST
    Figure CN118955780A_ABST
Patent Text Reader

Abstract

The invention discloses an antibacterial and deodorant super absorbent resin material and a preparation method thereof. According to the invention, the addition polymerization reaction is utilized to introduce the antibacterial monomer containing cations or zwitterions into the super absorbent resin, so that the super absorbent resin has a long-acting antibacterial function. An antibacterial group is introduced into the super absorbent resin through an addition polymerization reaction, so that the resin has long-term antibacterial performance, and also has a deodorization function due to the existence of a deodorization component. The super absorbent resin prepared by the method disclosed by the invention is high in water absorption speed, high in water absorption rate and good in saline water absorption performance, and integrates long-acting antibacterial performance and deodorization performance. The method can be applied to various fields of daily life, medical health and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer material modification and synthesis, and in particular relates to an antibacterial and deodorizing high water-absorbent resin material and a preparation method thereof. Background Art

[0002] Super absorbent resin is a special functional polymer material. It is a polymer with a three-dimensional network structure after proper cross-linking. It has water absorption and water retention properties because its three-dimensional structure contains strong water-absorbing groups such as carboxyl, amino, and hydroxyl. At present, more than 80% of super absorbent resins in the world are used in the field of disposable sanitary products. Super absorbent resins used in this field will directly contact the human body, and because the use environment is very easy for bacteria to breed, it is not good for health. In addition, excrement contains odor sources such as ammonia, and disposable sanitary products will produce odor during use, which stimulates the human body's olfactory senses and brings potential physiological and psychological harm to people. Therefore, it is of great significance to human health to develop a super absorbent resin with antibacterial and deodorizing functions for use in the field of disposable sanitary products.

[0003] There are also corresponding studies on antibacterial and deodorizing super absorbent resins in the existing technology. Patent CN114854161A "An antibacterial and deodorizing super absorbent resin and its preparation method" discloses an antibacterial and deodorizing super absorbent resin composite material. The super absorbent resin has excellent antibacterial and deodorizing properties. However, the antibacterial and deodorizing composite material is compounded on the super absorbent resin in the form of atomization, and there are problems such as unstable antibacterial and deodorizing components and easy dissolution, which cannot achieve a long-term antibacterial effect; Patent CN219099033U "An antibacterial and deodorizing super absorbent resin" uses tea powder The motherwort powder is an antibacterial deodorant, and a specific core-shell structure antibacterial and deodorizing super absorbent resin is prepared. The raw material composition and content are complex, and the preparation process of the core-shell structure super absorbent resin is difficult; Patent CN110862635A "An antibacterial and salt-resistant super absorbent resin and its preparation method and application" discloses an antibacterial and salt-resistant super absorbent resin and its preparation method and application. The method achieves the antibacterial effect by adding Ag-SiO2 composite antibacterial agent intercalated graphene antibacterial composition, but this type of release-type antibacterial material has poor antibacterial persistence and poor biological safety of inorganic antibacterial agents. Other studies simply achieve the effect of antibacterial deodorization by adding antibacterial ingredients. The antibacterial function can only reduce the generation of odor by inhibiting the reproduction of bacteria. However, the odor of the excrement itself cannot be eliminated by antibacterial agents, so this type of product cannot remove odor. Summary of the invention

[0004] In view of the problems of complex production process, poor antibacterial durability, poor biological safety of inorganic antibacterial agents, etc. of the current antibacterial and deodorizing super absorbent resin, the present invention designs and realizes a super absorbent resin with long-lasting antibacterial and deodorizing functions.

[0005] The purpose of the present invention is to provide a long-lasting antibacterial and deodorizing super absorbent resin and a preparation method thereof, by grafting cations or zwitterions on the three-dimensional structure of the super absorbent resin through addition polymerization, so that the super absorbent resin has a long-lasting antibacterial property, and adding a deodorizing component to make it have a deodorizing function. The shortcomings of the current super absorbent resin, such as short antibacterial cycle, low biological safety, and complex modification operation, are solved.

[0006] The highly absorbent resin prepared by the present invention has not only a long-lasting antibacterial function, but also has a deodorizing function due to the presence of deodorizing components, and can be applied to disposable sanitary products such as diapers and sanitary napkins.

[0007] The purpose of the present invention is achieved through the following technical solutions.

[0008] A method for preparing a highly absorbent resin having long-lasting antibacterial and deodorizing functions, specifically comprising the following preparation steps:

[0009] A certain amount of hydrophobic solvent and dispersant are added to a four-mouth open reactor equipped with a thermometer, condenser, overhead stirrer, and nitrogen glass tube, and heated to 40-50°C and stirred and dispersed for 15-30 minutes to obtain an oil phase. Acrylic acid is neutralized with sodium hydroxide solution under cold water bath conditions to obtain sodium acrylate solution, and antibacterial components and deodorizing components are added to the sodium acrylate solution to obtain an aqueous phase. The above-prepared aqueous phase is added to the reactor, and nitrogen is bubbled to drive oxygen. The temperature is raised to 60°C-80°C and heated and stirred for 1.5h-5h. During the polymerization process, the antibacterial monomer reacts with the resin to undergo an addition polymerization reaction, and the antibacterial material with cations and zwitterions is grafted onto the resin. Then, it is placed in an oven and dried at 80-120°C for 4-12h to obtain a highly absorbent resin for antibacterial and deodorizing.

[0010] The antibacterial component is an antibacterial monomer, specifically an antibacterial polymer generated by double bond free radical polymerization reaction initiated by an initiator from an olefin unsaturated monomer containing cations or zwitterions.

[0011] Furthermore, the olefin unsaturated monomer containing cations or zwitterions is one or more of methacryloyloxyethyl dimethylbenzyl ammonium chloride, sulfonate betaine methacrylate, carboxylate betaine methacrylate, acryloyloxyethyl trimethyl ammonium chloride, methacryloyloxyethyl trimethyl ammonium chloride, and N-(2-acryloyloxyethyl)-N-benzyl-N,N-dimethylammonium chloride. The mass of the olefin unsaturated monomer containing cations or zwitterions accounts for 1%-20% of the mass of acrylic acid.

[0012] Furthermore, in step (2), the cross-linking agent is one or more of N,N'-methylenebisacrylamide, polyethylene glycol diacrylate, and triethylene glycol dimethacrylate; the initiator is one or more of potassium persulfate, ammonium persulfate, and sodium bisulfite; in the aqueous phase solution, the cross-linking agent accounts for 0.5‰-3.0‰ of the total mass of the olefin unsaturated monomers containing cations or zwitterions, and the initiator accounts for 0.5‰-3‰ of the total mass of the olefin unsaturated monomers not containing cations or zwitterions.

[0013] Furthermore, the degree of neutralization of carboxyl groups in the sodium acrylate solution is 65%-85%.

[0014] Furthermore, the hydrophobic solvent is one or more of cyclohexane, n-hexane, cyclopentane, n-pentane, and petroleum ether.

[0015] Furthermore, the dispersant is one or more of Span 40, Span 60, Span 80, Tween 80, and OP-10. The mass of the dispersant component accounts for 0.5%-5% of the mass of the hydrophobic solvent.

[0016] Furthermore, the deodorizing component is one or more of graphene, activated carbon, yucca extract, red clover extract, and castor oil caprylate. The mass of the deodorizing component accounts for 0.4%-10% of the total mass of the olefin unsaturated monomer containing cations or zwitterions.

[0017] The highly water-absorbent resin with antibacterial and deodorizing properties of the present invention is prepared by the above method.

[0018] The antibacterial monomer with cationic groups used in the present invention has broad-spectrum antibacterial properties and a wide range of applications; the antibacterial monomer with cationic or anionic groups used in the present invention has low cytotoxicity and high antibacterial properties, especially the antibacterial monomer with a benzene ring structure can be assembled with graphene through π-π conjugation to make the two more closely combined, which has more significant advantages. At the same time, the deodorant component contains both an adsorbent and a urease inhibitor, which can absorb the odor source while inhibiting the generation of the odor source, and achieve a deodorizing effect by preventing the generation of odorous gas and absorbing and removing the odorous gas.

[0019] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0020] (1) The present invention introduces cationic or zwitterionic antibacterial groups into the super absorbent resin through addition polymerization reaction. Different from the conventional technical means in the field (directly adding antibacterial agents without chemical reactions), the super absorbent resin prepared by the method of the present invention has good bulk antibacterial properties and maintains the antibacterial properties of the material for a long time, and the antibacterial rate against Escherichia coli can reach more than 99%.

[0021] (2) The present invention uses an antibacterial monomer containing a benzene ring structure, which is assembled with graphene through π-π conjugation, so that the antibacterial monomer is more tightly combined with the resin, showing stronger antibacterial properties and better long-term sustained-release antibacterial properties.

[0022] (3) The antibacterial and deodorizing super absorbent resin of the present invention is safe and non-toxic, does not cause harm to the skin, has good antibacterial properties and liquid absorption properties, and can be applied to the field of disposable sanitary products.

[0023] (4) The antibacterial function of the super absorbent resin of the present invention is realized during the resin preparation process, and no secondary treatment of the resin is required. The preparation process is simple, which overcomes the complex process of the existing antibacterial super absorbent resin preparation that requires additional soaking, atomization spraying and drying, and the antibacterial substance is not easy to dissolve.

[0024] (5) The antibacterial and deodorizing super absorbent resin of the present invention can absorb the odor source while inhibiting the generation of the odor source, thereby achieving a deodorizing effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a graph showing the long-term antibacterial experimental test results of the antibacterial and deodorizing super absorbent resin prepared in Example 1.

[0026] Figure 2 This is a scanning electron microscope photograph of the morphology of the antibacterial and deodorizing super absorbent resin prepared in Example 1.

[0027] Figure 3 This is the Fourier infrared spectrum of the antibacterial and deodorizing super absorbent resin prepared in Example 3.

[0028] Figure 4 This is a graph showing the antibacterial experimental test results of the antibacterial and deodorizing super absorbent resin prepared in Comparative Example 1 and Example 1. DETAILED DESCRIPTION

[0029] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0030] Example 1

[0031] In a four-mouth open reactor equipped with a thermometer, condenser, overhead stirrer and nitrogen-permeated glass tube, 100 mL of cyclohexane, 0.72 g of Span60 and 0.73 g of OP-10 were added, heated to 50°C and stirred at 250 r / min for 15 min to uniformly disperse and obtain an oil phase. Take 9.72g of sodium hydroxide and dissolve it in 22.0g of distilled water, add 3.7g of distilled water to 23.1g of acrylic acid, then use sodium hydroxide solution to neutralize acrylic acid under cold water bath conditions to obtain sodium acrylate solution, then add 2.31g of antibacterial material methacryloyloxyethyl dimethylbenzyl ammonium chloride, 0.52g of deodorizing component graphene, 0.38g of yucca extract, 0.0438g of N,N'-methylenebisacrylamide, 0.0578g of potassium persulfate, and 0.0223g of sodium bisulfite to obtain an aqueous phase, add the above-prepared aqueous phase to the reactor, and at the same time, bubbling nitrogen to drive out oxygen, react at 50°C for 1h, then heat to 65°C for 1h, then continue to heat to 72°C for 3h, filter and dry at 110°C for 9h to obtain an antibacterial and deodorizing super absorbent resin.

[0032] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles", the antibacterial properties of super absorbent resin were tested by oscillation method, and the antibacterial rate of the resin against Escherichia coli was 99.1%. According to the current standard JISK7223-1996 "Test method for water absorption of super absorbent resin", the water absorption of the resin was tested, and the experimental results showed that the deionized water absorption rate of the resin was 495g / g.

[0033] Figure 1 The long-term antibacterial test result diagram of the long-term antibacterial super absorbent resin prepared in Example 1. After the resin was soaked in PBS buffer solution for different days, the antibacterial experiment was carried out on Escherichia coli. It can be seen that the antibacterial rates on the 1st, 3rd, 5th, 7th, 10th and 15th days of soaking in PBS buffer solution were 99.1%, 98.2%, 97.7%, 97.5%, 97.1% and 96.4% respectively. After a long period of soaking, the antibacterial rate only slightly decreased, indicating that the material still has excellent antibacterial performance after being soaked in PBS buffer solution for 15 days, and the material has long-term antibacterial properties.

[0034] Figure 2 This is a scanning electron microscope picture of the surface morphology of the antibacterial and deodorizing super absorbent resin prepared in Example 1. From the picture, it can be seen that the resin has a concave spherical structure and a rough surface structure. From the picture, it can be seen that a lot of flaky substances loaded on the surface of the resin are graphene, indicating that graphene has been successfully loaded on the surface of the resin, and it can be observed that the particle size of the resin is about 200 μm.

[0035] Example 2

[0036] In a four-mouth open reactor equipped with a thermometer, condenser, overhead stirrer and nitrogen-permeated glass tube, add 120 mL of cyclohexane, 1.02 g of Span60 and 0.38 g of Span80, heat to 45°C and stir at 250 r / min for 20 min to evenly disperse and obtain the oil phase. Take 10.42g of sodium hydroxide and dissolve it in 30.0g of distilled water, add 5.0g of distilled water to 25.1g of acrylic acid, then use sodium hydroxide solution to neutralize acrylic acid under cold water bath conditions to obtain sodium acrylate solution, then add 2.03g of antibacterial material methacryloyloxyethyl trimethyl ammonium chloride, 0.10g of deodorizing component graphene, 0.12g of yucca extract, 0.0252g of N,N'-methylenebisacrylamide, 0.0447g of potassium persulfate, and 0.0174g of sodium bisulfite to obtain an aqueous phase, add the above-prepared aqueous phase to the reactor, and at the same time, bubbling nitrogen to drive out oxygen, react at 45°C for 1h, then heat to 65°C for 1h, then continue to heat to 72°C for 2h, filter and dry at 100°C for 6h to obtain an antibacterial and deodorizing super absorbent resin.

[0037] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles", the antibacterial properties of super absorbent resin were tested by oscillation method, and the antibacterial rate of the resin against Escherichia coli was 98.6%. According to the current standard JISK7223-1996 "Test method for water absorption of super absorbent resin", the water absorption of the resin was tested, and the experimental results showed that the deionized water absorption rate of the resin was 453g / g.

[0038] Example 3

[0039] In a four-mouth open reactor equipped with a thermometer, a condenser, an overhead stirrer, and a nitrogen-permeated glass tube, 120 mL of cyclohexane and 1.52 g of Span60 were added, and the mixture was heated to 45°C and stirred at 250 r / min for 20 min to uniformly disperse the mixture to obtain an oil phase. Take 11.12g of sodium hydroxide and dissolve it in 30.0g of distilled water, add 5.0g of distilled water to 25.1g of acrylic acid, then use sodium hydroxide solution to neutralize acrylic acid under cold water bath conditions to obtain sodium acrylate solution, then add 1.25g of antibacterial material sulfonate betaine methacrylate, 0.15g of deodorizing component graphene, 0.0312g of N,N'-methylenebisacrylamide, 0.0498g of potassium persulfate, and 0.0193g of sodium bisulfite to obtain an aqueous phase, add the above-prepared aqueous phase to a reactor, and at the same time, bubbling nitrogen to drive out oxygen, react at 45°C for 1h, then heat to 55°C for 1h, then continue to heat to 72°C for 3h, filter and dry at 90°C for 6h to obtain an antibacterial and deodorizing super absorbent resin.

[0040] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles", the antibacterial properties of super absorbent resin were tested by oscillation method. The test showed that the antibacterial rate of the resin against Escherichia coli was 92.3%. According to the current standard JISK7223-1996 "Test method for water absorption of super absorbent resin", the water absorption of the resin was tested. The experimental results showed that the deionized water absorption rate of the resin was 547g / g.

[0041] Figure 3 This is the Fourier infrared spectrum of the antibacterial and deodorizing super absorbent resin prepared in Example 3. After the sulfobetaine methacrylate with antibacterial function is introduced into the super absorbent resin, it can be seen that at 1704 cm -1 The stretching vibration peak of C=O appears at 1055cm -1 The position corresponds to the asymmetric stretching vibration of the sulfonate anion group, which indicates that the antibacterial monomer sulfonate betaine methacrylate was successfully introduced into the polymer.

[0042] Example 4

[0043] In a four-mouth open reactor equipped with a thermometer, condenser, overhead stirrer and nitrogen-permeated glass tube, add 100 mL of cyclohexane, 1.02 g of Span60 and 0.47 g of Tween80, heat to 40°C and stir at 250 r / min for 30 min to evenly disperse and obtain the oil phase. Take 8.31g of sodium hydroxide and dissolve it in 20.0g of distilled water, add 4.4g of distilled water to 17.6g of acrylic acid, then neutralize the acrylic acid with sodium hydroxide solution under cold water bath conditions to obtain sodium acrylate solution, then add 1.88g of antibacterial material N-(2-acryloyloxyethyl)-N-benzyl-N,N-dimethylammonium chloride, 0.97g of deodorizing component graphene, 0.63g of red clover extract, 0.0503g of N,N'-methylenebisacrylamide, 0.0397g of potassium persulfate, and 0.0154g of sodium bisulfite to obtain an aqueous phase, add the above-prepared aqueous phase to the reactor, and at the same time, bubbling nitrogen to drive oxygen, react at 40°C for 1h, then heat to 65°C for 2h, and then continue to heat to 75°C for 1h, filter and dry at 120°C for 4h to obtain an antibacterial and deodorizing super absorbent resin.

[0044] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles", the antibacterial properties of super absorbent resin were tested by oscillation method, and the antibacterial rate of the resin against Escherichia coli was 99.3%. According to the current standard JISK7223-1996 "Test method for water absorption of super absorbent resin", the water absorption of the resin was tested, and the experimental results showed that the deionized water absorption rate of the resin was 510g / g.

[0045] Example 5

[0046] In a four-mouth open reactor equipped with a thermometer, condenser, overhead stirrer and nitrogen-permeated glass tube, add 140 mL of cyclohexane, 1.43 g of Span40 and 1.54 g of Tween80, heat to 50°C and stir at 250 r / min for 20 min to evenly disperse and obtain the oil phase. Take 5.64g of sodium hydroxide and dissolve it in 12.5g of distilled water, add 5.4g of distilled water to 12.71g of acrylic acid, then use sodium hydroxide solution to neutralize acrylic acid under cold water bath conditions to obtain sodium acrylate solution, then add 2.54g of antibacterial material acryloyloxyethyl trimethyl ammonium chloride, 0.59g of deodorizing component red clover extract, 0.68g of yucca extract, 0.0953g of N, N'-methylenebisacrylamide, 0.0318g of potassium persulfate, and 0.0123g of sodium bisulfite to obtain an aqueous phase, add the above-prepared aqueous phase to the reactor, and at the same time, bubbling nitrogen to drive out oxygen, react at 50°C for 1h, then heat to 70°C for 2h, then continue to heat to 80°C for 1h, filter and dry at 95°C for 9h to obtain an antibacterial and deodorizing super absorbent resin.

[0047] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles", the antibacterial properties of super absorbent resin were tested by oscillation method, and the antibacterial rate of the resin against Escherichia coli was 98.3%. According to the current standard JISK7223-1996 "Test method for water absorption of super absorbent resin", the water absorption of the resin was tested, and the experimental results showed that the deionized water absorption rate of the resin was 503g / g.

[0048] Example 6

[0049] In a four-mouth open reactor equipped with a thermometer, condenser, overhead stirrer and nitrogen-permeated glass tube, 120 mL of cyclohexane, 0.27 g of Span40 and 0.71 g of Span80 were added, heated to 45°C and stirred at 250 r / min for 20 min to uniformly disperse and obtain the oil phase. Take 15.47g of sodium hydroxide and dissolve it in 27.40g of distilled water, add 6.72g of distilled water to 32.77g of acrylic acid, then use sodium hydroxide solution to neutralize acrylic acid under cold water bath conditions to obtain sodium acrylate solution, then add 3.967g of antibacterial material carboxylic acid betaine methacrylate, 0.88g of deodorizing component activated carbon, 0.12g of graphene, 0.0410g of N,N'-methylenebisacrylamide, 0.0472g of ammonium persulfate, and 0.0182g of sodium bisulfite to obtain an aqueous phase, add the above-prepared aqueous phase to a reactor, and at the same time, bubbling nitrogen to drive out oxygen, react at 45°C for 1h, then heat to 75°C for 3h, filter and dry at 90°C for 12h to obtain an antibacterial and deodorizing super absorbent resin.

[0050] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles", the antibacterial properties of super absorbent resin were tested by oscillation method, and the antibacterial rate of the resin against Escherichia coli was 96.5%. According to the current standard JISK7223-1996 "Test method for water absorption of super absorbent resin", the water absorption of the resin was tested, and the experimental results showed that the deionized water absorption rate of the resin was 515g / g.

[0051] Comparative Example 1

[0052] In a four-mouth open reactor equipped with a thermometer, a condenser, an overhead stirrer, and a nitrogen-permeated glass tube, 100 mL of cyclohexane, 0.72 g of Span60, and 0.73 g of OP-10 were added, heated to 50°C, and stirred at 250 r / min for 15 min to uniformly disperse and obtain an oil phase. Take 9.72g of sodium hydroxide and dissolve it in 22.0g of distilled water, add 3.7g of distilled water to 23.1g of acrylic acid, and then neutralize the acrylic acid with sodium hydroxide solution under cold water bath conditions to obtain sodium acrylate solution, and then add 0.52g of deodorizing component graphene, 0.38g of yucca extract, 0.0438g of N,N'-methylenebisacrylamide, 0.0578g of ammonium persulfate, and 0.0223g of sodium bisulfite to obtain an aqueous phase, add the above-prepared aqueous phase to the reactor, and at the same time, bubbling nitrogen to drive oxygen, react at 50°C for 1h, then heat to 65°C for 1h, and then continue to heat to 72°C for 3h, filter and dry at 110°C for 9h to obtain a control group super absorbent resin.

[0053] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles", the antibacterial properties of the resin were tested by oscillation method. After testing, it was concluded that the resin had no antibacterial effect on Escherichia coli. According to the current standard JIS K7223-1996 "Test method for water absorption of super absorbent resin", the water absorption of the resin was tested. The experimental results showed that the deionized water absorption rate of the resin was 445g / g.

[0054] Figure 4 The figure is a test result of the antibacterial experiment of the water-absorbent resin prepared in Comparative Example 1 and Example 1. When the E. coli liquid is diluted to an appropriate multiple, the number of colonies in Comparative Example 1 (i.e., no antibacterial resin is added to the liquid) after 24 hours of cultivation is 211, and the number of colonies in Example 1 (i.e., the liquid is incubated with an antibacterial resin) after 24 hours of cultivation is reduced to 2, and the antibacterial rate is as high as 99.05%. The experimental results show that the highly absorbent resin prepared by the method of the present invention has a significant antibacterial effect.

[0055] Table 1 Performance test data of water-absorbent resin in various embodiments and comparative examples

[0056]

[0057] As shown in Table 1, the super absorbent resin prepared by the present invention not only has excellent antibacterial properties, but also has a high water absorption rate. At the same time, compared with Example 1 to Example 6, the antibacterial effect of the antibacterial monomer containing a benzene ring structure (Example 1 and Example 4) is better, because the antibacterial monomer containing a benzene ring structure is assembled with graphene through π-π conjugation, so that the antibacterial monomer is more closely combined with the resin, showing stronger antibacterial properties and better long-term sustained-release antibacterial properties, and the water absorption rate is also improved to a certain extent by introducing a carbonyl hydrophilic group through grafting. Taking into account the two factors of antibacterial properties and water absorption rate, the best embodiment is Example 4.

[0058] The present invention integrates the double bonds contained in the unsaturated monomer into the three-dimensional network structure of the resin through free radical reaction. On the one hand, the resin is given long-lasting and stable antibacterial activity. On the other hand, the anions and cations contained in the antibacterial monomer bind a large number of water molecules through electrostatic interaction to enhance the water absorption of the resin. Deodorizing properties are given to the resin by adding deodorizing substances.

[0059] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structural transformations made using the specification of the present invention, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A highly absorbent resin material for antibacterial and deodorizing functions and a method for preparing the same, It is characterized in that The specific preparation steps include: (1) adding a hydrophobic solvent and a dispersant into a four-mouth open reactor equipped with a thermometer, a condenser, an overhead stirrer, and a nitrogen-permeated glass tube, heating and stirring to disperse uniformly to obtain an oil phase; (2) neutralizing acrylic acid with sodium hydroxide solution in a cold water bath to obtain a sodium acrylate solution, and adding the antibacterial component and the deodorizing component as well as the crosslinking agent and the initiator to the sodium acrylate solution to obtain an aqueous phase; (3) Add the prepared aqueous phase into a reactor, while bubbling nitrogen to drive out oxygen, heating and stirring, and drying to obtain an antibacterial and deodorizing highly absorbent resin.

2. A method for preparing an antibacterial and deodorizing super absorbent resin according to claim 1, It is characterized in that In step (1), the hydrophobic solvent is one or more of cyclohexane, n-hexane, cyclopentane, n-pentane, and petroleum ether.

3. A method for preparing an antibacterial and deodorizing super absorbent resin according to claim 1, It is characterized in that In step (1), the dispersant is one or more of Span40, Span60, Span80, Tween80, OP-10; the mass of the dispersant accounts for 0.5%-5% of the mass of the hydrophobic solvent.

4. The method for preparing the antibacterial and deodorizing super absorbent resin according to claim 1, It is characterized in that In step (1), the heating and stirring is performed at a temperature of 40-50° C. and for a time of 15-30 min.

5. The method for preparing the antibacterial and deodorizing super absorbent resin according to claim 1, It is characterized in that In step (2), the antibacterial component is an antibacterial monomer, specifically an antibacterial polymer generated by a double bond free radical polymerization reaction initiated by an initiator through an olefin unsaturated monomer containing a cation or a zwitterion; the olefin unsaturated monomer containing a cation or a zwitterion is one or more of methacryloyloxyethyl dimethylbenzyl ammonium chloride, sulfonate betaine methacrylate, carboxylate betaine methacrylate, acryloyloxyethyl trimethyl ammonium chloride, methacryloyloxyethyl trimethyl ammonium chloride, and N-(2-acryloyloxyethyl)-N-benzyl-N,N-dimethylammonium chloride; the mass of the olefin unsaturated monomer containing a cation or a zwitterion accounts for 1%-20% of the mass of acrylic acid.

6. The method for preparing the antibacterial and deodorizing super absorbent resin according to claim 1, It is characterized in that In step (2), the cross-linking agent is one or more of N,N'-methylenebisacrylamide, polyethylene glycol diacrylate, and triethylene glycol dimethacrylate; the initiator is one or more of potassium persulfate, ammonium persulfate, and sodium bisulfite; in the aqueous phase solution, the cross-linking agent accounts for 0.5‰-3.0‰ of the total mass of the olefin unsaturated monomers containing cations or zwitterions, and the initiator accounts for 0.5‰-3‰ of the total mass of the olefin unsaturated monomers not containing cations or zwitterions.

7. The method for preparing the antibacterial and deodorizing super absorbent resin according to claim 1, It is characterized in that In step (2), the deodorizing component is one or more of graphene, activated carbon, yucca extract, red clover extract, and castor oil zinc ester; the mass of the deodorizing component accounts for 0.4%-10% of the total mass of the olefin unsaturated monomer containing cations or zwitterions.

8. The method for preparing the antibacterial and deodorizing super absorbent resin according to claim 1, It is characterized in that In step (3), the heating and stirring temperature is 60-80°C and the time is 1.5-5h.

9. The method for preparing the antibacterial and deodorizing super absorbent resin according to claim 1, It is characterized in that In step (3), the drying temperature is 80-120° C. and the drying time is 4-12 hours.

10. An antibacterial and deodorizing super absorbent resin prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Betaine antibacterial super absorbent polymer (SAP) and preparation method thereof

    CN103374093A

  • Antibacterial and deodorant high-water-absorbent resin and preparation method thereof

    CN105218734A

  • Preparation method of activated carbon modified polymer water-absorbent resin for astronaut paper diaper

    CN113354767A

  • Cat litter with deodorization and disinfection functions and preparation method thereof

    CN114651732A

  • Degradable antibacterial composite super absorbent resin and preparation method thereof

    CN116874690A

Cited By

  • Preparation method of antibacterial, deodorant and water-absorbent resin

    CN120399165A

  • Super absorbent resin and preparation method thereof

    CN121609842A