Delayed tackifying temperature-resistant and salt-resistant polymer for oil displacement and preparation method of delayed tackifying temperature-resistant and salt-resistant polymer
By introducing nano-silica into the polymer and optimizing process, a time-delayed viscosity-resistant and salt-resistant polymer was prepared, which solved the problem of lower viscosity under high temperature and high salt conditions, and improved the temperature resistance and salt resistance of the polymer. It is suitable for complex oilfield environments, reducing costs and reducing environmental pollution.
Patent Information
- Application Number
- CN202411314805.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-15
AI Technical Summary
The viscosity of existing temperature-resistant and salt-resistant polymers decreases under high temperature and high salt conditions, which leads to difficulty in injection wells and cannot effectively adjust the oil-water flow ratio, affecting the oil-to-water flow rate.
Using delayed viscosity-enhancing and temperature-resistant salt-resistant polymers, polymers with low initial viscosity at room temperature but gradually increase viscosity under specific temperature conditions through nano-silica, optimized cosolvents and polymerization conditions, and combined with glue blocks Process for cutting, freeze-drying, granulation and uniform distribution of nanomaterials.
It significantly improves the temperature resistance and salt resistance of polymers in high-temperature and high-salt environments, ensures the application and oil repellency of polymers in oil fields, reduces material and process costs, reduces environmental pollution, and is suitable for different Type of oil field.
Smart Images

Figure CN118955795A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oilfield oil recovery chemistry, and in particular relates to a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil recovery and a preparation method thereof. Background Art
[0002] Chemical flooding technology using partially hydrolyzed polyacrylamide (HPAM) as an oil displacement agent has become the leading technology for tertiary oil recovery in my country's oil fields. With the continuous development of high-temperature and high-salinity oil fields in my country, the viscosity of HPAM has been greatly reduced due to degradation, hydrolysis, precipitation, etc. under high-temperature and high-salinity conditions. In the field, the concentration of HPAM is generally increased to increase the viscosity of the polymer to meet the requirements of oil displacement in high-temperature and high-salinity reservoirs. However, high-concentration polymers will further lead to problems such as difficulty in injecting into the formation.
[0003] Therefore, in recent years, the research focus of heat-resistant and salt-resistant polymers at home and abroad has been concentrated on introducing functional monomers with special structural functional groups on the molecular chain to improve their heat-resistant and salt-resistant capabilities. Currently, a variety of new polymers such as hydrophobic associating, comb-type, and amphoteric have been developed. Field test results show that although heat-resistant and salt-resistant polymers can maintain high viscosity for a long time under high temperature and high mineralization formation conditions, their high viscosity polymers still have the problem of injection difficulties when injected into the well.
[0004] Therefore, it is urgent for those skilled in the art to develop a temperature-resistant and salt-resistant polymer with a delayed viscosity-increasing effect, so that the polymer has a low initial viscosity when prepared at room temperature, and after being injected into the well (under specific temperature conditions), its viscosity gradually increases with time. This will not affect the injection of the polymer, and after being injected into the formation, the viscosity can be increased, thereby effectively adjusting the oil-water mobility ratio and improving the recovery effect of polymer flooding.
[0005] In view of this, the inventors proposed a delayed viscosity-enhancing, temperature-resistant and salt-resistant polymer for oil displacement and a preparation method thereof to solve the above-mentioned problems. Summary of the invention
[0006] The object of the present invention is to provide a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A delayed viscosity-increasing, heat-resistant and salt-resistant polymer for oil displacement, the molecular formula of the delayed viscosity-increasing, heat-resistant and salt-resistant polymer for oil displacement is:
[0009]
[0010] Wherein, x is the degree of polymerization of acrylamide; y is the degree of polymerization of methylene acrylamide; and z is the degree of polymerization of phenyl acrylate.
[0011] Preferably, the ratio of y:z ranges from 2:1 to 1:2.
[0012] A method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement comprises the following steps:
[0013] S1. Mixing and dispersing: acrylamide, methylene acrylamide, phenyl acrylate, nano-silica, a cosolvent and deionized water are mixed in proportion, and stirred until completely dissolved and dispersed, and a pH adjuster is used to adjust the pH value to 6.5-7.5 to obtain a uniform dispersion;
[0014] S2, polymerization reaction, lowering the temperature of the dispersion obtained in step S1 to between 0 and 2° C. to ensure that the polymerization reaction proceeds slowly and evenly, introducing nitrogen for 35 to 50 minutes to ensure that dissolved oxygen in the system is completely eliminated, reduce the probability of redox side reactions, and maintain the stability of the reaction;
[0015] S3, using an initiator, adding a reducing agent with a mass fraction of 0.06% to 0.1%, and an oxidant with a mass fraction of 0.05% to 0.1%. During the polymerization initiation process, the reaction temperature is controlled within the range of 0 to 2°C. After adding the reducing agent and the oxidant, the reaction is maintained at a low temperature for 2 to 4 hours, and stirring is continued to ensure that the reaction is complete and a polymer is formed;
[0016] S4, heat preservation and aging. After the polymerization reaction is completed, the temperature is gradually increased to 50-60°C and kept for 4-6 hours for aging reaction to further improve the structural stability of the polymer;
[0017] S5. Post-processing, including block cutting, freeze drying, granulation and crushing, screening and uniform distribution of nanomaterials, improves the temperature and salt resistance of the final product.
[0018] Preferably, the contents of the components in step S1 are: 28% to 40% acrylamide, 1% to 10% methylene acrylamide, 1% to 10% phenyl acrylate, 0.5% to 2% nano-silica, 1.5% to 3% co-solvent, and the balance is deionized water.
[0019] Preferably, the co-solvent is ethylene glycol or pyrrolidone.
[0020] Preferably, the pH adjuster is an aqueous solution of sodium carbonate, sodium hydroxide or potassium hydroxide.
[0021] Preferably, the reducing agent in step S3 is sulfite or nitrite.
[0022] Preferably, the oxidant in step S3 is a peroxide or a persulfide.
[0023] Preferably, in step S5, the rubber block is cut, and after the polymer is formed, the polymer rubber block is taken out and cut;
[0024] Freeze drying: freeze drying is used to dry the cut polymer to keep the polymer structure intact;
[0025] Granulation and pulverization: The dried polymer is granulated by a granulator, and then the granules are pulverized by a pulverizer to ensure uniform distribution of particle size.
[0026] Preferably, the sieving in step S5 is to sieve polymer powders of different particle sizes by a sieving machine to ensure that a polymer product with uniform particle size is obtained, thereby improving the viscosity-increasing effect;
[0027] The nanomaterials are evenly distributed in the polymer through high-pressure homogenization technology to avoid agglomeration.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The present invention uses nanomaterials, adopts better co-solvents, adjusts polymerization conditions and improves post-treatment processes, which significantly improves the temperature resistance, salt resistance and viscosity-increasing effect of the polymer, and its particle distribution is more uniform, which is suitable for oil recovery operations in high-temperature and high-salt environments.
[0030] (2) The present invention adds nano-silicon dioxide to make the polymer have better high temperature resistance and salt resistance, which greatly improves the practicality of the polymer in high temperature and high salt oil field environment. The polymer can not only adapt to harsh environments such as high temperature and high salt, but also has excellent physical and chemical stability. It is suitable for the oil recovery needs of different types of oil fields, including conventional oil fields, deep well oil fields and heterogeneous oil reservoirs, which broadens its application prospects.
[0031] (3) The present invention adopts environmentally friendly cosolvents and mild polymerization conditions to reduce environmental pollution, reduce the negative impact on the oil field exploitation environment, and promote sustainable development. The optimized polymer has excellent temperature resistance, salt resistance and high-efficiency viscosity-increasing performance, which not only improves its application value in complex oil field environments, but also significantly reduces material and process costs, and has broad industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The molecular structure diagram of the delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement of the present invention;
[0033] Figure 2 This is a flow chart of a method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement according to the present invention;
[0034] Figure 3 It is a block diagram of the cosolvent composition of the present invention;
[0035] Figure 4 It is a block diagram of the pH adjusting agent composition of the present invention;
[0036] Figure 5 It is a block diagram of the reducing agent composition of the present invention;
[0037] Figure 6 It is a block diagram of the oxidant composition of the present invention. DETAILED DESCRIPTION
[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Embodiment 1:
[0040] See also Figures 1 to 6 As shown, a delayed viscosity-enhancing, heat-resistant and salt-resistant polymer for oil displacement, the molecular formula of the delayed viscosity-enhancing, heat-resistant and salt-resistant polymer for oil displacement is:
[0041]
[0042] Wherein, x is the degree of polymerization of acrylamide; y is the degree of polymerization of methylene acrylamide; and z is the degree of polymerization of phenyl acrylate.
[0043] Specifically, the ratio of y:z is 1:1.
[0044] A method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement comprises the following steps:
[0045] S1, mixing and dispersing, 28% acrylamide, 1% methylene acrylamide, 1% phenyl acrylate, 0.5% nano-silica, 1.5% cosolvent, and the rest deionized water are mixed, and stirred until completely dissolved and dispersed, and the pH value is adjusted to 6.5 with sodium carbonate aqueous solution to obtain a uniform dispersion;
[0046] S2, polymerization reaction, lowering the temperature of the dispersion obtained in step S1 to 0° C. to ensure that the polymerization reaction proceeds slowly and evenly, introducing nitrogen for 50 minutes to ensure that the dissolved oxygen in the system is completely eliminated, reduce the probability of redox side reactions, and maintain the stability of the reaction;
[0047] S3, using an initiator, adding 0.06% by mass of sodium bisulfite and 0.05% by mass of ammonium persulfate, during the polymerization initiation process, controlling the reaction temperature within the range of 0 to 2°C, adding the above-mentioned reducing agent and oxidizing agent, maintaining the low temperature reaction for 2 hours, and continuously stirring to ensure that the reaction is complete and a polymer is formed;
[0048] S4, heat preservation and aging. After the polymerization reaction is completed, the temperature is gradually increased to 50°C and kept for 6 hours for aging reaction to further improve the structural stability of the polymer;
[0049] S5. Post-processing, including block cutting, freeze drying, granulation and crushing, screening and uniform distribution of nanomaterials, improves the temperature and salt resistance of the final product.
[0050] Block cutting: after the polymer is formed, the polymer block is taken out and cut;
[0051] Freeze drying: freeze drying is used to dry the cut polymer to keep the polymer structure intact;
[0052] Granulation and pulverization: The dried polymer is granulated by a granulator, and then the granules are pulverized by a pulverizer to ensure uniform distribution of particle size.
[0053] Screening: use a screening machine to screen polymer powders of different particle sizes to ensure that polymer products with uniform particle sizes are obtained and improve the viscosity-increasing effect;
[0054] The nanomaterials are evenly distributed. Through high-pressure homogenization technology, at 50MPa and 70℃, the homogenization is performed for 30min to make the nanomaterials evenly distributed in the polymer and avoid agglomeration.
[0055] As can be seen from the above, the above-mentioned rubber block is taken out, cut, granulated, dried, crushed and sieved, and the parameters of the polyacrylamide polymer obtained can be specifically referred to as follows: 80-100 mesh, solid content 90.6%, hydrolysis degree 1.5%, dissolution and dispersion speed 60-80min, apparent viscosity 51mPa·s at 90°C and 50,000 mineralization, and apparent viscosity 2990mPa·s after being placed at 90°C for 30 days.
[0056] The viscometer used in the measurement process is a Brookfield DV-III model, with a No. 0 rotor (6 rpm), and the polyacrylamide product is in the form of white powder.
[0057] Embodiment 2:
[0058] See also Figures 1 to 6 As shown, a delayed viscosity-enhancing, heat-resistant and salt-resistant polymer for oil displacement, the molecular formula of the delayed viscosity-enhancing, heat-resistant and salt-resistant polymer for oil displacement is:
[0059]
[0060] Wherein, x is the degree of polymerization of acrylamide; y is the degree of polymerization of methylene acrylamide; and z is the degree of polymerization of phenyl acrylate.
[0061] Specifically, the ratio of y:z is 1:1.
[0062] A method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement comprises the following steps:
[0063] S1, mixing and dispersing, mixing acrylamide, methylene acrylamide, phenyl acrylate, nano-silica, a cosolvent and deionized water in proportion, stirring until completely dissolved and dispersed, and adjusting the pH value to 7.5 with a sodium carbonate aqueous solution to obtain a uniform dispersion;
[0064] S2, polymerization reaction, lowering the temperature of the dispersion obtained in step S1 to 2° C. to ensure that the polymerization reaction proceeds slowly and evenly, introducing nitrogen for 50 minutes to ensure that the dissolved oxygen in the system is completely eliminated, reduce the probability of redox side reactions, and maintain the stability of the reaction;
[0065] S3, using an initiator, adding 0.1% by mass of sodium bisulfite and 0.1% by mass of ammonium persulfate, during the polymerization initiation process, controlling the reaction temperature within the range of 0 to 2°C, adding the above-mentioned reducing agent and oxidizing agent, maintaining the low temperature reaction for 4 hours, and continuously stirring to ensure that the reaction is complete and a polymer is formed;
[0066] S4, heat preservation and aging, after the polymerization reaction is completed, the temperature is gradually increased to 60°C and kept for 6 hours for aging reaction to further improve the structural stability of the polymer;
[0067] S5. Post-processing, including block cutting, freeze drying, granulation and crushing, screening and uniform distribution of nanomaterials, improves the temperature and salt resistance of the final product.
[0068] Block cutting: after the polymer is formed, the polymer block is taken out and cut;
[0069] Freeze drying: freeze drying is used to dry the cut polymer to keep the polymer structure intact;
[0070] Granulation and pulverization: The dried polymer is granulated by a granulator, and then the granules are pulverized by a pulverizer to ensure uniform distribution of particle size.
[0071] Screening: use a screening machine to screen polymer powders of different particle sizes to ensure that polymer products with uniform particle sizes are obtained and improve the viscosity-increasing effect;
[0072] The nanomaterials are evenly distributed in the polymer through high-pressure homogenization technology at 50MPa and 70℃ for 30min to avoid agglomeration.
[0073] As can be seen from the above, the above-mentioned rubber block is taken out, cut, granulated, dried, crushed and sieved, and the parameters of the polyacrylamide polymer obtained can be specifically referred to as follows: 80-100 mesh, solid content 90.8%, hydrolysis degree 1.5%, dissolution and dispersion speed 60-80min, apparent viscosity 52mPa·s at 90°C and 50,000 mineralization, and apparent viscosity 2980mPa·s after being placed at 90°C for 30 days.
[0074] The viscometer used in the measurement process is a Brookfield DV-III model, with a No. 0 rotor (6 rpm), and the polyacrylamide product is a white powder.
[0075] Embodiment three:
[0076] This design is specifically applied to the oil extraction industry, specifically in deep well mining and the development of complex geological reservoirs. Deep well mining requires chemical oil displacement agents with higher temperature and pressure resistance. The modified polymer has excellent temperature and salt resistance, which is suitable for use in deep wells with complex geological conditions, extending the oil displacement cycle and improving the recovery rate. The heterogeneity of the reservoir requires the oil displacement agent to have good viscosity and diffusivity. The addition of nanomaterials in this design enhances the structural stability of the polymer, allowing it to cover the oil layer more evenly in the application of heterogeneous reservoirs and improve the recovery efficiency of the oil field.
[0077] Furthermore, a comparative example is set, specifically:
[0078] A method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement comprises the following steps:
[0079] S1, mixing and dispersing, mixing acrylamide, methylene acrylamide, phenyl acrylate, nano-silica, a co-solvent of benzenesulfonic acid and deionized water in proportion, stirring until completely dissolved and dispersed, adjusting the pH value to 6.5 with a sodium carbonate aqueous solution, and obtaining a uniform dispersion;
[0080] S2, polymerization reaction, lowering the temperature of the dispersion obtained in step S1 to between 0 and 2° C. to ensure that the polymerization reaction proceeds slowly and evenly, introducing nitrogen for 40 minutes to ensure that dissolved oxygen in the system is completely eliminated, reduce the probability of redox side reactions, and maintain the stability of the reaction;
[0081] S3, using an initiator, adding a reducing agent with a mass fraction of 0.1%, and an oxidant with a mass fraction of 0.1%. During the polymerization initiation process, the reaction temperature is controlled within a range of 5°C. After adding the reducing agent and the oxidant, the reaction is maintained at a low temperature for 4 hours, and stirring is continued to ensure that the reaction is complete and a polymer is formed;
[0082] S4, heat preservation and aging, after the polymerization reaction is completed, the temperature is gradually increased to 60°C and kept for 4 hours for aging reaction to further improve the structural stability of the polymer;
[0083] S5. Post-processing, including block cutting, freeze drying, granulation and crushing, screening and uniform distribution of nanomaterials, improves the temperature and salt resistance of the final product.
[0084] Specifically, the contents of the components in step S1 are: 28% acrylamide, 5% methylene acrylamide, 7% phenyl acrylate, 1% nano-silica, 2% co-solvent, and the balance is deionized water.
[0085] Specifically, in step S5, after the polymer is formed, the polymer block is taken out and cut;
[0086] Freeze drying: freeze drying is used to dry the cut polymer to keep the polymer structure intact;
[0087] Granulation and pulverization: The dried polymer is granulated by a granulator, and then the granules are pulverized by a pulverizer to ensure uniform distribution of particle size.
[0088] Specifically, in step S5, the polymer powders of different particle sizes are screened by a screening machine to ensure that a polymer product with uniform particle size is obtained, thereby improving the viscosity-increasing effect;
[0089] The nanomaterials are evenly distributed in the polymer through high-pressure homogenization technology to avoid agglomeration.
[0090] The data obtained by testing Example 1 and the comparative example are shown in Table 1 below:
[0091]
[0092]
[0093] Table 1
[0094] It can be seen from the above table that the technical solution adopted by the present invention has the following effects:
[0095] Viscosity enhancement: The viscosity of the polymer in Example 1 at room temperature and high temperature is significantly higher than that of the polymer prepared by the traditional method, indicating that the introduction of nano-silica and the optimization of polymerization conditions enhance the viscosity-enhancing effect of the polymer.
[0096] Temperature resistance: Under a high temperature environment of 80°C, the viscosity of Example 1 is well maintained, and the viscosity decreases slightly, which is about 54% higher than that of traditional polymers. This shows that the addition of nano-silica effectively enhances the temperature resistance of the polymer.
[0097] Salt resistance: In a solution containing 3% NaCl, Example 1 has better salt resistance and higher viscosity retention rate, with the viscosity increased by about 38%, indicating that the use of nanomaterials and ethylene glycol as a cosolvent can improve the salt resistance of the polymer.
[0098] High temperature and high salt environment: Under high temperature and high salt environment, the viscosity of Example 1 is still better than that of Example 3, and the viscosity is increased by about 72%, indicating that the viscosity-enhancing, temperature-resistant and salt-resistant polymer prepared by the technical solution of the present invention is more suitable for oil displacement needs under harsh environments.
[0099] Particle size distribution: The average particle size of Example 1 is 60 μm, which is more uniform than 90 μm of the traditional method, indicating that the freeze-drying and ultrasonic dispersion processes effectively reduce the agglomeration of polymer particles and improve their dispersibility.
[0100] Conclusion: The use of nanomaterials, better cosolvents, adjustment of polymerization conditions and improvement of post-treatment processes have significantly improved the temperature resistance, salt resistance and viscosity-increasing effect of the polymer, and its particle distribution is more uniform, making it suitable for oil recovery operations in high temperature and high salt environments.
[0101] From the above, we can see that by adding nano-silica, the polymer has better high temperature resistance and salt resistance, which greatly improves the practicality of the polymer in high temperature and high salt oil field environment. The polymer can not only adapt to harsh environments such as high temperature and high salt, but also has excellent physical and chemical stability. It is suitable for the oil recovery needs of different types of oil fields, including conventional oil fields, deep well oil fields and heterogeneous oil reservoirs, broadening its application prospects.
[0102] The use of environmentally friendly cosolvents and mild polymerization conditions reduces environmental pollution, can reduce the negative impact on the oil field exploitation environment, and promote sustainable development. The optimized polymer, with its excellent temperature resistance, salt resistance and efficient viscosity increasing performance, not only improves its application value in complex oil field environments, but also significantly reduces material and process costs, and has broad industrial application prospects.
[0103] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory.
[0104] In the drawings of the embodiments disclosed in the present invention, only the structures related to the embodiments disclosed in the present invention are involved, and other structures can refer to the general design. In the absence of conflict, the same embodiment and different embodiments of the present invention can be combined with each other.
[0105] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement, It is characterized in that The molecular formula of the delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement is: Wherein, x is the degree of polymerization of acrylamide; y is the degree of polymerization of methylene acrylamide; and z is the degree of polymerization of phenyl acrylate.
2. A delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement according to claim 1, Features: The y:z ratio ranges from 2:1 to 1:
2.
3. A method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement according to any one of claims 1 to 2, It is characterized in that The following steps are involved: S1. Mixing and dispersing: acrylamide, methylene acrylamide, phenyl acrylate, nano-silica, a cosolvent and deionized water are mixed in proportion, and stirred until completely dissolved and dispersed, and a pH adjuster is used to adjust the pH value to 6.5-7.5 to obtain a uniform dispersion; S2, polymerization reaction, lowering the temperature of the dispersion obtained in step S1 to between 0 and 2° C. to ensure that the polymerization reaction proceeds slowly and evenly, introducing nitrogen for 35 to 50 minutes to ensure that dissolved oxygen in the system is completely eliminated, reduce the probability of redox side reactions, and maintain the stability of the reaction; S3, using an initiator, adding a reducing agent with a mass fraction of 0.06% to 0.1%, and an oxidant with a mass fraction of 0.05% to 0.1%. During the polymerization initiation process, the reaction temperature is controlled within the range of 0 to 2°C. After adding the reducing agent and the oxidant, the reaction is maintained at a low temperature for 2 to 4 hours, and stirring is continued to ensure that the reaction is complete and a polymer is formed; S4, heat preservation and aging. After the polymerization reaction is completed, the temperature is gradually increased to 50-60°C and kept for 4-6 hours for aging reaction to further improve the structural stability of the polymer; S5. Post-processing, including block cutting, freeze drying, granulation and crushing, screening and uniform distribution of nanomaterials, improves the temperature and salt resistance of the final product.
4. A method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement according to claim 3, Features: The contents of the components in step S1 are: 28% to 40% acrylamide, 1% to 10% methylene acrylamide, 1% to 10% phenyl acrylate, 0.5% to 2% nano-silicon dioxide, 1.5% to 3% cosolvent, and the balance is deionized water.
5. The method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement according to claim 3, Features: The cosolvent is ethylene glycol or pyrrolidone.
6. A method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement according to claim 3, Features: The pH adjuster is an aqueous solution of sodium carbonate, sodium hydroxide or potassium hydroxide.
7. The method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement according to claim 3, Features: In step S3, the reducing agent is sulfite or nitrite.
8. The method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement according to claim 3, Features: In step S3, the oxidant is a peroxide or a persulfide.
9. The method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement according to claim 3, Features: In step S5, the polymer block is cut, and after the polymer is formed, the polymer block is taken out and cut; Freeze drying: freeze drying is used to dry the cut polymer to keep the polymer structure intact; Granulation and pulverization: The dried polymer is granulated by a granulator, and then the granules are pulverized by a pulverizer to ensure uniform distribution of particle size.
10. The method for preparing a delayed viscosity-increasing, temperature-resistant and salt-resistant polymer for oil displacement according to claim 3, Features: Screening in step S5, using a screening machine to screen polymer powders of different particle sizes to ensure that a polymer product with uniform particle size is obtained and improve the viscosity-increasing effect; The nanomaterials are evenly distributed in the polymer through high-pressure homogenization technology to avoid agglomeration.