Low-temperature early-strength water reducing agent and preparation method thereof
By introducing a variety of functional groups into early strength polycarboxylic acid water reducing agents and the application of biomass materials, the problem of early strength improvement of concrete in low temperature environments is solved, and efficient water reduction and early strength effects are achieved, simplifying the Process and reduce environmental impact.
Patent Information
- Application Number
- CN202411007546.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The existing early strength polycarboxylic acid water reducing agent cannot effectively improve the early strength of concrete in low temperature environments, and the traditional synthesis methods have by-product uncertainty and process complexity, which limits its application in low temperature environments.
Through amidation, esterification, Michael addition, free radical polymerization and Thiol-ene reaction, low-temperature premature water reducing agents containing a variety of functional groups are designed and synthesized, and natural polymer chitosan and trehalose are used to produce biochemical products such as chitosan and trehalose. Material materials form a new molecular structure with excellent water reduction and early strength effects.
In low temperature environments, the early strength and water reduction effect of concrete are significantly improved, the impact on the ecosystem is reduced, the synthesis process is simplified, suitable for industrial promotion, and the construction performance and economic benefits of concrete are improved.
Smart Images

Figure CN118955813A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of water reducing agents, and in particular to a low-temperature early-strength water reducing agent and a preparation method thereof. Background Art
[0002] In recent years, with the acceleration of infrastructure construction in my country and the rapid development of industries such as real estate, concrete, as the largest consumable in the building materials industry, has been widely used in many fields. In addition, with the development of reinforcement and maintenance projects, the production of precast concrete parts and the advancement of national housing industrialization, new requirements have been put forward for the early strength of concrete. Especially for cold areas, the low-temperature construction of ready-mixed concrete is a common problem faced by northern my country. During the transition period between winter construction and normal construction, temperature fluctuations will lead to great uncertainty in the development of concrete strength. Due to the low ambient temperature, traditional concrete has problems such as poor working performance and collapse resistance and slow early strength development, which seriously affects the construction progress of concrete. Therefore, it is urgent to develop an admixture that can effectively improve the working performance of concrete and increase its early strength in a low temperature environment.
[0003] At present, the research field promotes the development of early strength of concrete by reducing water-cement ratio, using high-strength cement, using high-quality sand and gravel aggregates, and adding early strength agents. Among them, early strength agents are considered to be one of the most widely used measures to promote the development of early strength of concrete due to their low cost, simple operation, and good early strength improvement effect.
[0004] There are many types of early strength agents, which can be divided into inorganic salt early strength agents, organic early strength agents, and composite early strength agents (composite of inorganic and organic substances) according to their chemical composition. Inorganic salt early strength agents mainly include chlorides (such as calcium chloride, etc.), sulfates, nitrates, nitrites, carbonates, lithium salts, nanomaterials and crystal embryos, etc. Organic early strength agents mainly include alcoholamines (such as triethanolamine and triisopropanolamine, etc.), calcium formate, urea and early strength polycarboxylic acid water reducers, etc. Composite early strength agents mainly include chlorides and alcoholamines, carbonates and alcoholamines, inorganic salts and early strength polycarboxylic acid water reducers, etc. Although inorganic salt early strength agents can improve the early strength of concrete, the Cl contained in them - 、SO4 2- and CO3 2-It will increase the shrinkage of concrete, aggravate the corrosion of steel bars, and seriously affect the durability of concrete. Organic early strength agents are mainly some small organic molecules. Their action mechanism is relatively simple, and the effect of improving the early strength of concrete is poor and expensive. In addition, some early strength polycarboxylate water reducers can improve the early strength of concrete at room temperature, but they cannot play an early strength effect in low temperature environments. Therefore, the development of low-temperature early strength water reducers suitable for low-temperature curing environments, with good working performance and good early strength improvement effects, is of great practical significance for solving the problem of the development of early strength of concrete in cold regions.
[0005] The natural high molecular polymer chitosan used in the present invention contains a large number of amino groups, and the molecular designability is strong. A long polymer chain with multiple amide groups is obtained by amide reaction and Michael addition reaction, and then a polymer containing imide is obtained by free radical polymerization with polyether macromonomers, olefinic acid small monomers and sulfonic acid small monomers, and then an olefin-functionalized polymer is obtained by Hofmann degradation reaction and amidation reaction. The presence of olefin enables it to serve as a contact point for Thiol-ene reaction. Therefore, if a monomer with multiple hydroxyl groups is grafted on the basis of the olefin-functionalized polymer through Thiol-ene reaction to form a molecular structure with multiple hydroxyl groups, the synergistic effect of carboxyl, sulfonic acid, amide and hydroxyl groups is achieved, and the freezing point of the pore solution inside the concrete is effectively reduced, which innovatively breaks through the poor working performance of the traditional early-strength polycarboxylic acid water-reducing agent under low-temperature environment and the insignificant early strength improvement effect.
[0006] Chinese invention patent CN117304422A (publication date: December 29, 2023) reports an early-strength polycarboxylic acid water-reducing agent and a preparation method thereof, which is copolymerized at room temperature by unsaturated sulfonic acid monomers, unsaturated esterification monomers, unsaturated carboxylic acid monomers, initiators and solvents. The invention uses epoxy silane coupling agent and double-terminal silicone oil to carry out dealcoholization reaction to obtain an epoxy-terminated modifier, and then reacts with a saturated monobasic organic acid to obtain a silicon-modified esterification product containing hydroxyl groups, and then reacts with an allyl epoxy-terminated polyether containing an amino group and a silyl group to produce an epoxy ring-opening reaction. The advantage of this invention is that the synthesized early-strength water-reducing agent has good dispersibility for cement particles, high water reduction rate, and good early strength effect. However, the functional group that plays an early strength role in this invention is only the sulfonic acid group, the number of functional groups is small, and the type is relatively single, and the effect of improving the early strength of concrete under low temperature environment has not yet been carried out.
[0007] Chinese invention patent CN117126346A (publication date: November 28, 2023) reports a crystal core early strength polycarboxylic acid water reducer and its preparation method. The invention uses a one-step synthesis process, using unsaturated carboxylic acids, unsaturated amides, ethylene glycol monovinyl polyoxyethylene ether, oxidants, reducing agents, chain transfer agents and modified crystal core free radical polymerization. The advantage of this invention is that it adopts a one-pot synthesis method, which can improve the early strength of concrete, improve the discharging state of concrete, and has good dispersibility and plasticity for mortar. However, the invention does not significantly improve the early strength of concrete by relying solely on modified crystal cores, and whether it is effective in developing the early strength of concrete in a low temperature environment remains to be investigated.
[0008] Chinese invention patent CN116535580A (publication date: August 4, 2023) reports a polyether end-functionalized ultra-early strength polycarboxylic acid water reducer and its preparation method. The invention prepares a modified polyether macromonomer with terminal hydroxyl grafted carboxyl groups by alcoholysis of cyclic dianhydride, and then reacts with aminosiloxane for amidation to prepare a modified polyether with a long-chain branched end group having an amino group and a silane ring structure, which is then copolymerized with amide monomer free radicals. The advantage of this invention is that the synthesis process is simple and easy to operate, and it has a certain promoting effect on the development of early strength of concrete. However, the invention is not purified in the alcoholysis reaction, amidation reaction and free radical polymerization reaction process, and the final synthesized sample may contain some by-products. The unknown product ratio brings greater uncertainty to subsequent applications.
[0009] The early-strength polycarboxylate water-reducing agents described in most existing patents have a certain improvement effect on the working performance of concrete and can promote the development of early strength of concrete to a certain extent, proving that the synthesized early-strength polycarboxylate water-reducing agents with sulfonic acid groups and amide groups can significantly improve the application efficacy of polymers. However, the above-mentioned synthesis methods all have certain shortcomings. Researchers mostly focus on modifying traditional polycarboxylate water-reducing agents. It is difficult to significantly improve the early strength of concrete by simply introducing groups or modifying polyether side chains. Moreover, most patents only focus on the study of the effect of improving the early strength of concrete under normal temperature conditions. In low-temperature curing environments, many water-reducing agents lose their activity, making it difficult to promote the development of early strength of concrete under low-temperature conditions, which limits their promotion and application under low-temperature conditions. Therefore, it is urgent to develop a low-temperature early-strength water reducer with a new molecular structure. It is necessary to innovatively synthesize a water reducer containing carboxyl, sulfonic acid, amide and hydroxyl groups based on the molecular structure design concept, and accurately control the molecular structure of the low-temperature early-strength water reducer through the synthesis methods of amidation, esterification, Michael addition, free radical polymerization, Hofmann degradation and Thiol-ene reaction, so that the synthesized low-temperature early-strength water reducer can not only play the role of water reduction, but also ensure the reduction of the freezing point of the concrete pore solution to promote the development of the early strength of the concrete. The synthesis method is easy to control, which is conducive to industrial promotion. There are no relevant reports on this work at home and abroad. Summary of the invention
[0010] In view of this, the present invention provides a low-temperature early-strength water reducer and a preparation method thereof, wherein the monomers obtained by amidation reaction and esterification reaction are subjected to Michael addition reaction to obtain a polyester macromonomer, and then free radical polymerization reaction is carried out with a polyether macromonomer, a carboxylic acid small monomer and a sulfonic acid small monomer, and then functional modification is carried out through Hofmann degradation and amidation reaction in sequence, and then Thiol-ene reaction is carried out with thiolated trehalose to synthesize a low-temperature early-strength water reducer, so as to solve the problems existing in the prior art.
[0011] In order to achieve the above object, the present invention adopts the following technical solution:
[0012] The present invention provides a low-temperature early-strength water reducer, and the structural formula of the low-temperature early-strength water reducer is as follows:
[0013]
[0014] Among them, the structural formula of R' is:
[0015]
[0016] Among them, the wavy line position is the connection position, R is CH2, CH2CH2 or O(CH2CH2O)2, R1 is H, CH3, CH2CH3 or CH2COOH, R2 is H or CH3, R3 is H, OH, CH3O, Cl or Br, R4 is H, OH, CH3O or Cl, and R5 is H or Na; a, b, c, d, m, n, x and f are integers, indicating the number of repeating units of each part in the polymer, a is 10 to 150, b is 3 to 40, c is 3 to 30, d is 3 to 50, m is 0 to 100, n is 10 to 150, x is 2 to 10, and f is 1 to 5.
[0017] The present invention also provides a method for preparing the low-temperature early-strength water-reducing agent, comprising the following steps:
[0018] (1) dissolving chitosan in solvent 1 to obtain mixed solution 1; activating unsaturated carboxylic acid small monomer, solvent 2 and activator to obtain mixed solution 2; adding mixed solution 2 to mixed solution 1 to carry out amidation reaction, and then dialyzing and vacuum drying in sequence to obtain amidated product 1;
[0019] (2) reacting poly(ethylene glycol) methacrylate, bipyridine and solvent 3 to obtain a mixed solution 3; mixing N,N'-disuccinimidyl carbonate, a pyridine compound and solvent 4 and adding the mixture to the mixed solution 3 to carry out an esterification reaction, and then successively performing reduced pressure distillation and purification to obtain an esterification product;
[0020] (3) reacting the amidation product 1 with the solvent 1 to obtain a mixed solution 4; dissolving the esterification product in the solvent 5 and then dropwise adding the mixture to the mixed solution 4 to perform a Michael addition reaction, followed by dialysis and vacuum drying to obtain a Michael addition product;
[0021] (4) The polyether macromonomer and solvent 5 are mixed to obtain a bottom liquid, an oxidant is first added to the bottom liquid and stirred evenly, and then liquid A, liquid B and liquid C are simultaneously added to the bottom liquid; wherein liquid A is a mixture of olefinic acid small monomer, sulfonic acid small monomer and solvent 5, liquid B is a mixture of Michael addition product and solvent 5, and liquid C is a reducing agent, a chain transfer agent and Solvent 5 After the dropwise addition is completed, a free radical polymerization reaction is carried out, and a free radical polymerization product is obtained by distillation under reduced pressure;
[0022] (5) subjecting the free radical polymerization product, the catalyst, the solvent 6 and the alkaline solution to a Hofmann degradation reaction, followed by purification and vacuum drying to obtain a Hofmann degradation product;
[0023] (6) reacting the Hofmann degradation product with solvent 5 to obtain a mixed solution 6; dissolving the anhydride small monomer in solvent 7 and heating it in a water bath to obtain a mixed solution 7; subjecting the mixed solution 6, the mixed solution 7 and the amine small monomer to an amidation reaction, followed by dialysis and vacuum drying to obtain an amidated product 2;
[0024] (7) Trehalose, triphenylphosphine and solvent 4 are mixed, and an amine compound is added dropwise thereto to carry out reaction 1. After reaction 1 is completed, an ester substance and an alcohol substance are added thereto in sequence to carry out reaction 2, followed by extraction, washing and vacuum drying to obtain thiolated trehalose; amidation product 2 is reacted with solvent 4 to obtain a mixed solution 8; thiolated trehalose is dissolved in solvent 2, and solvent 8 is added to mix well, and the mixed solution is added to the mixed solution 8 to carry out a Thiol-ene reaction, and then the mixture is cooled to room temperature and purified in sequence to obtain a low-temperature early-strength water reducer.
[0025] In step (1) of the present invention, solvent 1 includes acetic acid or hydrochloric acid, and the mass concentration of solvent 1 is 0.5-2%; the unsaturated carboxylic acid small monomer includes cinnamic acid, m-chlorocinnamic acid, m-bromocinnamic acid, p-chlorocinnamic acid, p-bromocinnamic acid, caffeic acid or 3,4-dimethoxycinnamic acid; solvent 2 includes phosphate buffer; the activator includes 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide The molar ratio of imide is 1-2:1; the molar ratio of chitosan and unsaturated carboxylic acid small monomer is 1-2:1; the molar ratio of activator and unsaturated carboxylic acid small monomer is 2-4:1; the mass ratio of solvent 1, solvent 2 and chitosan is 40-60:20-40:1; the dissolution temperature is 20-30°C, and the dissolution time is 12-24h; the activation temperature is 20-30°C, and the activation time is 1-3h; the amidation reaction temperature is 30-35°C, and the amidation reaction time is 2-6h.
[0026] In step (2) of the present invention, solvent 3 includes water or anhydrous ethanol; the pyridine compound includes pyridine, 4-dimethylaminopyridine or 2-bromo-4-dimethylaminopyridine; solvent 4 includes one or more of N,N-dimethylformamide, N,4-dimethylformamide and dimethyl sulfoxide; the molar ratio of poly(ethylene glycol) methacrylate, bipyridine, N,N'-disuccinimidyl carbonate and pyridine compound is 10-40:1:30-60:40-60; the mass ratio of poly(ethylene glycol) methacrylate, solvent 3 and solvent 4 is 1:30-60:40-80; the reaction is carried out under nitrogen conditions, and the reaction time is 10-30 minutes; the esterification reaction is carried out under nitrogen conditions, the esterification reaction temperature is 70-90°C, and the esterification reaction time is 4-6 hours.
[0027] In step (3) of the present invention, solvent 1 includes acetic acid or hydrochloric acid, and the mass concentration of solvent 1 is 0.5-2%; solvent 5 is water; the molar ratio of esterification product and amidation product 1 is 0.5-1:1; the mass ratio of amidation product 1, solvent 1 and solvent 5 is 1:60-120:40-80; the reaction is carried out under nitrogen conditions, the reaction temperature is 30-50°C, and the reaction time is 1-3h; the dropwise addition time is 40-80min; the Michael addition reaction is carried out under nitrogen conditions, the Michael addition reaction temperature is 50-70°C, and the Michael addition reaction time is 20-24h.
[0028] In step (4) of the present invention, the polyether macromonomer includes methyl allyl polyoxyethylene ether, isopentanol polyethoxyethylene ether or butanediol monovinyl polyoxyethylene ether, and the molecular weight of the polyether macromonomer is 2000-5000 g / mol; the solvent 5 independently includes water; the oxidant includes H2O2, ammonium persulfate, potassium persulfate or sodium persulfate; the olefinic acid small monomer includes acrylic acid, methacrylic acid, 2-ethylacrylic acid, maleic anhydride, itaconic acid, crotonic acid, crotonic anhydride, isomethacrylic acid or trans-2-pentenoic acid; the sulfonic acid small monomer includes 2-acrylamide-2-methylpropanesulfonic acid or 2-methyl-2-[(1-oxo-2-propenyl)amino]-1-propanesulfonic acid sodium salt; the reducing agent includes one or more of ascorbic acid, bleaching powder and FeSO4; the chain transfer agent includes thioglycolic acid, 3-mercaptopropionic acid, sodium hypophosphite, sodium allylpropanesulfonate or sodium methacrylic acid; the polyether The molar ratio of the macromonomer to the olefinic acid small monomer is 1:4-8; the molar ratio of the oxidant, the olefinic acid small monomer, the sulfonic acid small monomer, the Michael addition product, the reducing agent and the chain transfer agent is 0.03-0.1:1:0.035-0.1:0.035-0.1:0.003-0.01:0.01-0.2; during the mixing process of the polyether macromonomer and the solvent 5, the mass ratio of the polyether macromonomer to the solvent 5 is 1:20-160; the ratio of the total mass of the olefinic acid small monomer and the sulfonic acid small monomer in liquid A to the mass of the solvent 5 is 1:10-40; the mass ratio of the Michael addition product to the solvent 5 in liquid B is 1:10-20; the ratio of the total mass of the reducing agent and the chain transfer agent in liquid C to the mass of the solvent 5 is 1:10-20; the dripping time is 40-80 minutes; the temperature of the free radical polymerization reaction is 20-70°C, and the time of the free radical polymerization reaction is 2-6 hours.
[0029] In step (5) of the present invention, the catalyst comprises one or more of silver chloride, cuprous bromide, bromine, sodium chlorite, and sodium bromite; the solvent 6 comprises anhydrous ethanol or water; the alkaline solution comprises one or more of a NaOH aqueous solution, a KOH aqueous solution, and an NH4OH aqueous solution, and the mass concentration of the alkaline solution is 4-6%; the molar ratio of the free radical polymerization product to the catalyst is 10-20:1; the mass ratio of the free radical polymerization product, the solvent 6, and the alkaline solution is 1:30-100:20-40; the Hofmann degradation reaction comprises a first-stage Hofmann degradation reaction and a second-stage Hofmann degradation reaction; the parameters of the first-stage Hofmann degradation reaction are as follows: argon gas conditions, a temperature of 20-30°C, and a time of 30-50 min; the parameters of the second-stage Hofmann degradation reaction are as follows: argon gas conditions, a temperature of 120-180°C, and a time of 4-8 h.
[0030] In step (6) of the present invention, solvent 5 is water; the anhydride small monomer includes nadic anhydride or cis-5-naphthene-exo-2,3-dicarboxylic anhydride; solvent 7 includes one or more of tetrahydrofuran, benzene, toluene, methanol, ethanol, isopropanol, and n-butanol, and the mass concentration of solvent 7 is 4-6%; the amine small monomer includes ethylenediamine, tetramethylenediamine, 1,4-butanediamine, 1,6-hexanediamine, 1,8-octanediamine or decanediamine; Hofmann degradation products and anhydrides The molar ratio of the small monomer is 1 to 4:1; the molar ratio of the Hofmann degradation product, the solvent 7 and the amine small monomer is 1:1 to 2:1 to 2; the mass ratio of the Hofmann degradation product and the solvent 5 is 1:40 to 60; the reaction temperature is 20 to 30°C, and the reaction time is 4 to 8 hours; the water bath heating temperature is 40 to 60°C, and the water bath heating time is 0.5 to 1 hour; the amidation reaction temperature is 20 to 30°C, and the amidation reaction time is 12 to 24 hours.
[0031] In step (7) of the present invention, the solvent 4 independently includes one or more of N,N-dimethylformamide, N,4-dimethylformamide, and dimethyl sulfoxide; the amine compound includes N-bromosuccinimide and / or N-hydroxysuccinimide; the ester substance includes ethyl acetate, ethyl propionate, ethyl butyrate, ethyl isobutyrate, ethyl valerate or ethyl isovalerate; the alcohol substance includes DL-dithiothreitol, dithiothreitol, dithioerythritol, L-1,4-dithiothreitol, 1,2-butanedithiol, 1,4-butanedithiol, 2,3-butanedithiol, 1,6-hexanedithiol thiol, 1,2-ethanedithiol or 1,5-pentanedithiol; solvent 2 includes phosphate buffer; solvent 8 includes one or more of 240-260 mg / ml methanol, 0.01-0.03 w / v% eosin, and 0.1-0.3 v / v% triethanolamine; the molar ratio of trehalose to triphenylphosphine is 0.2-0.8:1; the molar ratio of trehalose to alcohol substances is 1:2-4; the molar ratio of triphenylphosphine, amine compounds and ester substances is 1:1-2:1-3; the molar ratio of amidation product 2 to thiolated trehalose is 2-4:1; solvent 2, solvent 8 and The mass ratio of thiolated trehalose is 20-40:5-20:1; during the mixing process of trehalose, triphenylphosphine and solvent 4, the mass ratio of solvent 4 to trehalose is 30-60:1; in the mixed solution 8, the mass ratio of solvent 4 to amidation product 2 is 10-40:1; the dropwise addition time is 1-2 hours; the temperature of reaction 1 is 20-30°C, and the reaction time is 36-48 hours; the temperature of reaction 2 is 20-30°C, and the reaction time is 12-24 hours; the reaction temperature is 20-30°C, and the reaction time is 12-24 hours; the Thiol-ene reaction includes The reactants are sequentially subjected to a first-stage Thiol-ene reaction, a pH value adjustment and a second-stage Thiol-ene reaction; the parameters of the first-stage Thiol-ene reaction are as follows: nitrogen conditions, ultraviolet light irradiation, a temperature of 20 to 30°C, and a time of 12 to 24 hours; the pH adjuster used for adjusting the pH value includes one or more of phosphate buffer, oxalic acid, acetic acid, and citric acid, and the pH value is adjusted to 6 to 8; the parameters of the second-stage Thiol-ene reaction are as follows: nitrogen conditions, ultraviolet light irradiation, a temperature of 30 to 40°C, and a time of 10 to 30 minutes.
[0032] In steps (1) to (7) of the present invention, the dialysis is independently performed using a dialysis bag, and the dialysis time is independently 48 to 72 hours; the vacuum drying time is independently 24 to 48 hours; the temperature of the reduced pressure distillation is independently 100 to 115°C; the extraction agent used for the extraction includes one or more of benzene, toluene, xylene, and chloroform; and the cleaning reagent includes anhydrous ethanol.
[0033] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0034] 1. The present invention is based on the theory of molecular structure design. Unsaturated carboxylic acid small monomers and polyester macromonomers are introduced into the natural high molecular polymer chitosan by the method of "amide + esterification + Michael addition", and then free radical polymerization is carried out with polyether macromonomers, carboxylic acid small monomers and sulfonic acid small monomers to obtain a polymer containing two long side chains, which increases the steric hindrance effect of the polymer, and then functional modification is carried out by amidation reaction, and then Thiol-ene reaction is carried out with thiolated trehalose to synthesize a low-temperature early strength water reducer. The molecular structure of the low-temperature early strength water reducer contains a large number of carboxyl groups, sulfonic acid groups, amide groups and hydroxyl groups. The synergistic effect of these functional groups enables the low-temperature early strength water reducer to show excellent water reduction effect and significantly improve the early strength of concrete under low temperature environment. Compared with the existing early strength polycarboxylic acid water reducer on the market, the water reduction and early strength effect under low temperature environment are better, which is an innovation and breakthrough in the direction of early strength polycarboxylic acid water reducer, and opens up new ideas and directions for the subsequent development of low-temperature early strength water reducer.
[0035] 2. Based on the development concept of green environmental protection, the present invention applies biomass materials such as natural high molecular weight polymer chitosan, unsaturated carboxylic acid (such as cinnamic acid and its derivatives), trehalose and other materials to the synthesis and preparation of low-temperature early strength water reducer, realizing the combination of biomass materials and the diversity needs of concrete admixtures. At the same time, copolymerization with traditional polyether macromonomers to synthesize low-temperature early strength water reducer can further enhance the water reduction and early strength effects of traditional early strength polycarboxylic acid water reducer in low temperature or even negative temperature environment. This is not only conducive to solving the problems of poor concrete working performance and slow early strength development in low temperature or negative temperature environment, but also effectively reduces the impact and damage to the ecosystem, and is also conducive to the industrial promotion and application of low temperature early strength water reducer.
[0036] 3. The present invention is based on the water reduction and early strength action principle of low-temperature early strength water reducer. After copolymerizing unsaturated carboxylic acid small monomers with polyether macromonomers, sulfonic acid small monomers and polyester macromonomers, thiolated trehalose containing a large number of hydroxyls is introduced to synthesize low-temperature early strength water reducer. The presence of a large number of carboxyl groups can improve its adsorption capacity for cement particles as a whole, and play an excellent water reduction effect. The presence of sulfonic acid groups can improve the dispersibility of cement paste and promote the hydration of C3A in cement to play an early strength effect. The presence of a large number of hydroxyls can produce a hydrogen bond network that destroys the hydrogen bond network that causes water to freeze in a low temperature environment, so that the early strength of concrete in a low temperature or even negative temperature environment can also be improved. At the same time, the polyether side chain and the polyester side chain can produce a strong steric hindrance, so that the cement particles repel each other and disperse, so that the prepared low-temperature early strength water reducer has an excellent water reduction and dispersion effect.
[0037] 4. Compared with the traditional early-strength polycarboxylate water-reducing agent, the present invention introduces biomass materials, reduces the use of petroleum-based polyether macromonomers, significantly reduces the preparation cost of low-temperature early-strength water-reducing agent, and the raw materials are green, environmentally friendly, non-toxic and harmless, avoiding the harm to the environment and human body caused by excessive use of toxic materials. The low-temperature early-strength water-reducing agent prepared by the present invention has a more significant effect of reducing water and strengthening early than the early-strength polycarboxylate water-reducing agent with a single functional group through the synergistic effect of multiple functional groups. At the same time, the reaction steps such as amidation, esterification, Michael addition, free radical copolymerization, Hofmann degradation, Thiol-ene, etc. used in the present invention belong to common preparation processes, do not require special equipment conditions and process flows, are conducive to industrial production of products, and have broad application prospects.
[0038] 5. From the perspective of engineering application, the low-temperature early-strength water-reducing agent prepared by the present invention has good stability, and no stratification, deterioration and precipitation occur during long-term storage. It also has the characteristics and performance advantages of high water reduction rate and excellent early-strength effect. It has good working performance and collapse resistance when applied to concrete in low-temperature or even negative-temperature environments, and can meet the requirements of long-distance transportation. At the same time, the early strength develops quickly, the construction quality is high, the turnover rate of the formwork is improved, and the problems of inability to construct normally in low-temperature or even negative-temperature environments, severe concrete freezing damage, and slow development of early strength of concrete are solved. It has significant economic benefits, performance advantages and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0040] Figure 1 This is the infrared spectrum test diagram of the low-temperature early-strength water-reducing agent obtained in Example 1. DETAILED DESCRIPTION
[0041] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0042] Example 1
[0043] (1) Amidation reaction: Chitosan was dissolved in 1% acetic acid solution, stirred at 20°C for 24 hours, cinnamic acid was dissolved in phosphate buffer, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide were added, stirred at 25°C for 1 hour, and then added to the chitosan solution, stirred at 30°C for 4 hours, dialyzed with a dialysis bag for 48 hours to remove unreacted solvent and small molecules, and vacuum dried for 48 hours to obtain an amidation product. (Wherein, the molar ratio of chitosan, cinnamic acid, 1-ethyl-(3-dimethylaminopropyl)carbodiimide, and N-hydroxysuccinimide is 2:1:2:2, and the mass ratio of acetic acid, phosphate buffer, and chitosan is 60:40:1)
[0044] (2) Esterification reaction: Add poly(ethylene glycol) methacrylate, bipyridine and anhydrous ethanol to a reactor, introduce N2, stir for 10 min, add N,N'-disuccinimidyl carbonate and 4-dimethylaminopyridine to N,N-dimethylformamide, stir evenly, then add to the reactor, continue to introduce N2, stir at 90°C for 4 h, distill under reduced pressure at 100°C, purify, and obtain an esterification product. (Wherein, the molar ratio of poly(ethylene glycol) methacrylate, bipyridine, N,N'-disuccinimidyl carbonate, and 4-dimethylaminopyridine is 40:1:40:40, and the mass ratio of anhydrous ethanol, N,N-dimethylformamide, and poly(ethylene glycol) methacrylate is 40:60:1)
[0045] (3) Michael addition reaction: The amidation product obtained in step (1) and 1% acetic acid are added to a reactor, N2 is introduced, and the reaction is stirred at 30°C for 1 hour. Subsequently, the esterification product obtained in step (2) is dissolved in deionized water and then added dropwise to the reactor within 50 minutes, and then stirred for 24 hours in a 50°C N2 environment, dialyzed for 48 hours, and vacuum dried for 48 hours to obtain a Michael addition product. (Wherein, the esterification product: amidation product = 0.5:1, and the mass ratio of acetic acid, deionized water, and amidation product is 60:40:1)
[0046] (4) Free radical polymerization reaction: add methyl allyl polyoxyethylene ether with a molecular weight of 2400 g / mol and deionized water into a reactor and stir evenly to obtain a bottom liquid, first add H2O2 into the bottom liquid and stir evenly, then simultaneously add liquid A, liquid B and liquid C into the bottom liquid within 50 min; wherein liquid A is a mixture of acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid and water, liquid B is a mixture of Michael addition product and water, and liquid C is a mixture of bleaching powder, FeSO4, 3-mercaptopropionic acid and water; after the addition is completed, stir the reaction at 65°C for 2 h, and remove the solvent and by-products by vacuum distillation to obtain a free radical polymerization product. (Wherein, the molar ratio of methyl allyl polyoxyethylene ether, H2O2, acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid, Michael addition product, bleaching agent, FeSO4, and 3-mercaptopropionic acid is 1:0.3:5:0.175:0.2:0.02:0.015:0.1, the mass ratio of deionized water and methyl allyl polyoxyethylene ether is 80:1, the mass ratio of the total mass of acrylic acid and 2-acrylamide-2-methylpropane sulfonic acid in liquid A to the mass ratio of water is 1:20, the mass ratio of Michael addition product to water in liquid B is 1:10, and the mass ratio of the total mass of bleaching agent, FeSO4, and 3-mercaptopropionic acid in liquid C to water is 1:10)
[0047] (5) Hofmann degradation reaction: The free radical polymerization product obtained in step (4), sodium chlorite, anhydrous ethanol and 5% NaOH aqueous solution are added to a reactor, argon is introduced, and the mixture is stirred at 20° C. for 45 min, then the mixture is heated to 150° C. and stirred for 5 h, purified, and vacuum dried for 48 h to obtain a Hofmann degradation product. (Wherein, the molar ratio of the free radical polymerization product to sodium chlorite is 10:1, and the mass ratio of anhydrous ethanol to NaOH solution to the free radical polymerization product is 50:30:1)
[0048] (6) Amidation reaction: The Hofmann degradation product obtained in step (5) and deionized water are added to a reactor, stirred and reacted at 20° C. for 4 hours, and then nadic anhydride is dissolved in 5% tetrahydrofuran, heated in a constant temperature water bath at 40° C. for 0.5 hours, and then added to the reactor, and ethylenediamine is added, stirred and reacted at 20° C. for 18 hours, dialyzed for 48 hours, and vacuum dried for 48 hours to obtain an amidation product. (Wherein, the molar ratio of Hofmann degradation product, nadic anhydride, tetrahydrofuran, and ethylenediamine is 2:1:2:2, and the mass ratio of deionized water to Hofmann degradation product is 50:1)
[0049] (7) Thiol-ene reaction: trehalose, triphenylphosphine and N,N-dimethylformamide are added to a reactor, N-bromosuccinimide is added dropwise for 1 hour, the mixture is stirred and reacted at 20°C for 40 hours, ethyl acetate and DL-dithiothreitol are added in sequence, the mixture is stirred and reacted at 20°C for 12 hours, the mixture is extracted with toluene, washed with anhydrous ethanol, and vacuum dried for 48 hours to obtain thiolated trehalose; subsequently, the amidated product obtained in step (6) and N,N-dimethylformamide are added to a reactor, the mixture is stirred and reacted at 20°C for 12 hours, the thiolated trehalose is dissolved in phosphate buffer, 250 mg / ml methanol solution is added, the mixture is stirred and added to the reactor, N2 is introduced, the mixture is stirred and reacted at 20°C for 12 hours under ultraviolet light, phosphate buffer is added, the pH value of the solution is adjusted to 6-8, the mixture is stirred and reacted at 30°C for 20 minutes, the mixture is cooled to room temperature, and purified to obtain a low-temperature early strength water reducer. (Wherein, the molar ratio of trehalose, triphenylphosphine, N-bromosuccinimide, ethyl acetate, and DL-dithiothreitol is 0.4:1:1:2:2, the mass ratio of N,N-dimethylformamide and trehalose is 50:1; the molar ratio of amidation product and thiolated trehalose is 2:1, and the mass ratio of anhydrous dimethylformamide, phosphate buffer, methanol, and sulfated trehalose is 50:40:15:1).
[0050] Example 2
[0051] (1) Amidation reaction: Chitosan was dissolved in a 1.5% hydrochloric acid solution, stirred at a constant temperature of 25°C for 16 hours, and then caffeic acid was dissolved in a phosphate buffer solution, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide were added, stirred and activated at 25°C for 2 hours, and then added to the chitosan solution, stirred and reacted at 30°C for 4 hours, dialyzed using a dialysis bag for 48 hours to remove unreacted solvents and small molecules, and vacuum dried for 48 hours to obtain an amidation product. (Wherein, the molar ratio of chitosan, caffeic acid, 1-ethyl-(3-dimethylaminopropyl)carbodiimide, and N-hydroxysuccinimide is 2:1:3:3, and the mass ratio of hydrochloric acid, phosphate buffer, and chitosan is 50:40:1)
[0052] (2) Esterification reaction: Add poly(ethylene glycol) methacrylate, bipyridine and deionized water into a reactor, introduce N2, stir for 20 min, add N,N'-disuccinimidyl carbonate and pyridine into N,N-dimethylformamide, stir evenly, then add into the reactor, continue to introduce N2, stir at 80°C for 6 h, distill under reduced pressure at 110°C, purify, and obtain an esterification product. (Wherein, the molar ratio of poly(ethylene glycol) methacrylate, bipyridine, N,N'-disuccinimidyl carbonate, and pyridine is 30:1:35:40, and the mass ratio of deionized water, N,N-dimethylformamide, and poly(ethylene glycol) methacrylate is 50:50:1)
[0053] (3) Michael addition reaction: The amidation product obtained in step (1) and 1% hydrochloric acid are added to a reactor, N2 is introduced, and the reaction is stirred at 40°C for 2 hours. Subsequently, the esterification product obtained in step (2) is dissolved in deionized water and then added dropwise to the reactor within 45 minutes, and then stirred for 24 hours in a 60°C N2 environment, dialyzed for 48 hours, and vacuum dried for 48 hours to obtain a Michael addition product. (Wherein, the esterification product: amidation product = 0.8:1, and the mass ratio of hydrochloric acid, deionized water, and amidation product is 70:40:1)
[0054] (4) Free radical polymerization reaction: add isopentanol polyethoxylate ether with a molecular weight of 2400 g / mol and deionized water into a reactor and stir evenly to obtain a bottom liquid, first add ammonium persulfate into the bottom liquid, and then add liquid A, liquid B and liquid C to the bottom liquid at the same time within 55 minutes; wherein liquid A is a mixture of itaconic acid, 2-methyl-2-[(1-oxo-2-propenyl)amino]-1-propanesulfonic acid sodium salt and water, liquid B is a mixture of Michael addition product and water, and liquid C is a mixture of ascorbic acid, thioglycolic acid and water; after the addition is completed, stir the reaction at 50°C for 5 hours, and remove the solvent and by-products by vacuum distillation to obtain a free radical polymerization product. (Wherein, the molar ratio of prenol polyethoxylate, ammonium persulfate, itaconic acid, 2-methyl-2-[(1-oxo-2-propenyl)amino]-1-propanesulfonic acid sodium salt, Michael addition product, ascorbic acid, and thioglycolic acid is 1:0.3:6:0.24:0.3:0.024:0.3, the mass ratio of deionized water and prenol polyethoxylate is 100:1, the mass ratio of the total mass of acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid in liquid A to water is 1:20, the mass ratio of the Michael addition product to water in liquid B is 1:10, and the total mass ratio of ascorbic acid and thioglycolic acid to water in liquid C is 1:15)
[0055] (5) Hofmann degradation reaction: The free radical polymerization product obtained in step (4), cuprous bromide, deionized water and 5% NaOH aqueous solution were added to a reactor, argon was introduced, and the reaction was stirred at 25°C for 40 minutes, then the temperature was raised to 140°C and stirred for 6 hours, purified, and vacuum dried for 48 hours to obtain a Hofmann degradation product. (Wherein, the molar ratio of the free radical polymerization product to cuprous bromide was 15:1, and the mass ratio of deionized water, NaOH solution, and the free radical polymerization product was 60:35:1)
[0056] (6) Amidation reaction: The Hofmann degradation product obtained in step (5) and deionized water are added to a reactor, stirred and reacted at 25° C. for 5 hours, then cis-5-norbornene-exo-2,3-dicarboxylic anhydride is dissolved in a 5% methanol solution, heated in a constant temperature water bath at 45° C. for 0.5 hours, and then added to the reactor, and tetramethylenediamine is added, stirred and reacted at 25° C. for 15 hours, dialyzed for 48 hours, and vacuum dried for 48 hours to obtain an amidation product. (Wherein, the molar ratio of Hofmann degradation product, cis-5-norbornene-exo-2,3-dicarboxylic anhydride, methanol, and tetramethylenediamine is 3:1:4.5:3, and the mass ratio of deionized water to Hofmann degradation product is 60:1)
[0057] (7) Thiol-ene reaction: trehalose, triphenylphosphine and N,N-dimethylformamide are added to a reactor, N-hydroxysuccinimide is added dropwise for 1.5 hours, the mixture is stirred and reacted at 25°C for 36 hours, ethyl butyrate and dithiothreitol are added in sequence, the mixture is stirred and reacted at 25°C for 12 hours, the mixture is extracted with toluene, washed with anhydrous ethanol, and vacuum dried for 48 hours to obtain thiolated trehalose; subsequently, the amidated product obtained in step (6) and N,N-dimethylformamide are added to a reactor, the mixture is stirred and reacted at 25°C for 12 hours, the thiolated trehalose is dissolved in phosphate buffer, 0.02 w / v% eosin solution is added, the mixture is stirred and added to the reactor, N2 is introduced, the mixture is stirred and reacted at 25°C under ultraviolet light for 16 hours, phosphate buffer is added, the pH value of the solution is adjusted to 6-8, the mixture is stirred and reacted at 35°C for 25 minutes, the mixture is cooled to room temperature, and purified to obtain a low-temperature early strength water reducer. (Wherein, the molar ratio of trehalose, triphenylphosphine, N-hydroxysuccinimide, ethyl butyrate and dithiothreitol is 0.5:1:2:2:3, the mass ratio of N,N-dimethylformamide and trehalose is 50:1; the molar ratio of amidation product and thiolated trehalose is 2.5:1, and the mass ratio of N,N-dimethylformamide, phosphate buffer, eosin and sulfated trehalose is 60:40:20:1).
[0058] Example 3
[0059] (1) Amidation reaction: Chitosan was dissolved in a 1% hydrochloric acid solution, stirred at a constant temperature of 30°C for 12 hours, 3,4-dimethoxycinnamic acid was dissolved in a phosphate buffer, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide were added, stirred at 25°C for 1.5 hours for activation, and then added to the chitosan solution, stirred at 30°C for 5 hours, dialyzed with a dialysis bag for 48 hours to remove the unreacted solvent and small molecules, and vacuum dried for 48 hours to obtain an amidation product. (Wherein, the molar ratio of chitosan, 3,4-dimethoxycinnamic acid, 1-ethyl-(3-dimethylaminopropyl)carbodiimide, and N-hydroxysuccinimide is 2:1.5:2:2, and the mass ratio of hydrochloric acid, phosphate buffer, and chitosan is 55:40:1)
[0060] (2) Esterification reaction: Add poly(ethylene glycol) methacrylate, bipyridine and deionized water into a reactor, introduce N2, stir for 25 min, add N,N'-disuccinimidyl carbonate and 2-bromo-4-dimethylaminopyridine into dimethyl sulfoxide, stir evenly, add into the reactor, continue to introduce N2, stir at 85°C for 4 h, distill under reduced pressure at 105°C, purify, and obtain an esterification product. (Wherein, the molar ratio of poly(ethylene glycol) methacrylate, bipyridine, N,N'-disuccinimidyl carbonate, 2-bromo-4-dimethylaminopyridine is 45:1:40:40, and the mass ratio of deionized water, dimethyl sulfoxide, poly(ethylene glycol) methacrylate is 55:60:1)
[0061] (3) Michael addition reaction: The amidation product obtained in step (1) and 1% acetic acid are added to a reactor, N2 is introduced, and the reaction is stirred at 45°C for 1.5 hours. Subsequently, the esterification product obtained in step (2) is dissolved in deionized water and then added dropwise to the reactor within 60 minutes, and then stirred for 20 hours in a 65°C N2 environment, dialyzed for 72 hours, and vacuum dried for 48 hours to obtain a Michael addition product. (Wherein, the esterification product: amidation product = 0.8:1, and the mass ratio of acetic acid, deionized water, and amidation product is 80:60:1)
[0062] (4) Free radical polymerization reaction: Butanediol monovinyl polyoxyethylene ether with a molecular weight of 5000 g / mol and deionized water are added to a reactor and stirred evenly to obtain a bottom liquid. Potassium persulfate is first added to the bottom liquid, and then liquid A, liquid B and liquid C are simultaneously added dropwise to the bottom liquid within 60 minutes; wherein liquid A is a mixture of methacrylic acid, 2-acrylamido-2-methylpropane sulfonic acid and water, liquid B is a mixture of Michael addition product and water, and liquid C is a mixture of ascorbic acid, sodium allylpropane sulfonate and water; after the addition is completed, the mixture is stirred and reacted at 20° C. for 5 hours, and the solvent and by-products are removed by reduced pressure distillation to obtain a free radical polymerization product. (Wherein, the molar ratio of polyoxyethylene butylene glycol monovinyl ether, potassium persulfate, methacrylic acid, 2-acrylamide-2-methylpropane sulfonic acid, Michael addition product, ascorbic acid, and sodium allyl formate is 1:0.42:7:0.315:0.315:0.03:0.28, the mass ratio of deionized water and polyoxyethylene butylene glycol monovinyl ether is 120:1, the mass ratio of the total mass of acrylic acid and 2-acrylamide-2-methylpropane sulfonic acid in liquid A to water is 1:15, the mass ratio of the Michael addition product in liquid B to water is 1:15, and the mass ratio of the total mass of ascorbic acid and sodium allyl formate in liquid C to water is 1:10)
[0063] (5) Hofmann degradation reaction: The free radical polymerization product obtained in step (4), sodium bromite, deionized water and 5% NaOH aqueous solution were added to a reactor, argon was introduced, and the mixture was stirred at 30°C for 35 minutes, then heated to 150°C and stirred for 4 hours, purified, and vacuum dried for 48 hours to obtain a Hofmann degradation product. (Wherein, the molar ratio of the free radical polymerization product to sodium bromite was 18:1, and the mass ratio of deionized water, NaOH solution, and the free radical polymerization product was 80:30:1)
[0064] (6) Amidation reaction: The Hofmann degradation product obtained in step (5) and deionized water are added to a reactor, stirred and reacted at 30° C. for 4 hours, and then nadic anhydride is dissolved in a 5% ethanol solution, heated in a constant temperature water bath at 50° C. for 1 hour, and then added to the reactor, and 1,6-hexanediamine is added, stirred and reacted at 30° C. for 12 hours, dialyzed for 48 hours, and vacuum dried for 48 hours to obtain an amidation product. (Wherein, the molar ratio of Hofmann degradation product, nadic anhydride, ethanol, and 1,6-hexanediamine is 2:1:3.5:3.5, and the mass ratio of deionized water to Hofmann degradation product is 50:1)
[0065] (7) Thiol-ene reaction: trehalose, triphenylphosphine and dimethyl sulfoxide are added to a reactor, N-bromosuccinimide is added dropwise for 2 hours, the mixture is stirred and reacted at 30°C for 40 hours, ethyl propionate and dithioerythritol are added in sequence, the mixture is stirred and reacted at 30°C for 12 hours, the mixture is extracted with xylene, washed with anhydrous ethanol, and vacuum dried for 48 hours to obtain thiolated trehalose; subsequently, the amidated product obtained in step (6) and dimethyl sulfoxide are added to a reactor, the mixture is stirred and reacted at 30°C for 12 hours, the thiolated trehalose is dissolved in phosphate buffer, 0.2 v / v% triethanolamine is added, the mixture is stirred and added to the reactor, N2 is introduced, the mixture is stirred and reacted at 30°C under ultraviolet light for 15 hours, phosphate buffer is added, the pH value of the solution is adjusted to 6-8, the mixture is stirred and reacted at 30°C for 20 minutes, the mixture is cooled to room temperature, and purified to obtain a low-temperature early strength water reducer. (Wherein, the molar ratio of trehalose, triphenylphosphine, N-bromosuccinimide, ethyl propionate, and dithioerythritol is 0.6:1:1.5:2:4, the mass ratio of dimethyl sulfoxide and trehalose is 55:1; the molar ratio of amidation product and thiolated trehalose is 3:1, and the mass ratio of dimethyl sulfoxide, phosphate buffer, triethanolamine, and sulfated trehalose is 55:35:20:1)
[0066] Comparative Example 1
[0067] ViscoCrete-W early-strength polycarboxylate water-reducing agent commercially available from Sika Company was used as comparative example 1.
[0068] Comparative Example 2
[0069] The KS-4 early-strength polycarboxylate water-reducing agent commercially available from Guangdong Shuangta New Materials Co., Ltd. was used as Comparative Example 2.
[0070] Comparative Example 3
[0071] The YB-513 early-strength polycarboxylate water-reducing agent commercially available from Shaanxi Youbang New Material Technology Co., Ltd. was used as Comparative Example 3.
[0072] Effect and performance testing:
[0073] 1. Fluidity of cement paste:
[0074] In order to investigate the effect of the low-temperature early-strength water-reducing agent synthesized in the present invention on the fluidity of cement paste, the fluidity of cement pastes mixed with the low-temperature early-strength water-reducing agent prepared in Examples 1 to 3 and the early-strength polycarboxylate water-reducing agent prepared in Comparative Examples 1 to 3 was tested according to GB / T 8077 under the same water-reducing agent dosage and water-cement ratio. In the test, W / C=0.29:1, and the water-reducing agent dosage was 0.15% of the cement mass (solid ratio). The examples used were cement pastes mixed with the low-temperature early-strength water-reducing agent synthesized in Examples 1 to 3 of the present invention, and the comparative examples used were cement pastes mixed with the early-strength polycarboxylate water-reducing agent prepared in Comparative Examples 1 to 3. The test results of cement paste fluidity are shown in Table 1.
[0075] Table 1 Cement paste fluidity test results
[0076]
[0077]
[0078] It can be seen from Table 1 that compared with the early-strength polycarboxylate water-reducing agent of Comparative Examples 1 to 3, the low-temperature early-strength water-reducing agent prepared in Examples 1 to 3 can significantly improve the fluidity of the cement paste, and after 1h and 2h of time loss, the fluidity retention performance of the cement paste mixed with the low-temperature early-strength polycarboxylate water-reducing agent prepared in Examples 1 to 3 is better than the fluidity retention performance of the cement paste mixed with the early-strength polycarboxylate water-reducing agent of Comparative Examples 1 to 3, indicating that the low-temperature early-strength water-reducing agent exhibits excellent dispersibility and cement adaptability.
[0079] 2. Concrete performance:
[0080] In this test, concrete with strength grade C30 was selected, and its mix ratio is shown in Table 2. Among them, the cement used is Chengde Jinyu P·O 42.5 cement, the sand is II zone continuous graded natural medium sand with fineness modulus of 2.8 and mud content less than 2.1%, the stone is 5-20mm continuous graded crushed stone, the dosage of low temperature early strength water reducer is 0.2% of the mass of cementitious material (solid ratio), and the molding and curing of concrete specimens are carried out according to GB / T 50081. The examples used are concretes mixed with the low temperature early strength water reducer synthesized in Examples 1 to 3 of the present invention, and the comparative examples used are concretes mixed with the early strength polycarboxylate water reducer of Comparative Examples 1 to 3.
[0081] Table 2C30 concrete mix ratio (kg / m 3 )
[0082] cement Fly ash sand gravel water 290 60 760 1150 150
[0083] (1) Concrete slump and expansion:
[0084] In order to investigate the effect of the low-temperature early-strength water reducing agent synthesized by the present invention on the working performance of concrete, the proportions of the various components of the concrete were controlled to be the same, and the slump, expansion and slump / expansion loss over time of the concretes added with different embodiments and comparative examples were tested according to GB 8076. The test results are shown in Table 3.
[0085] Table 3 Concrete slump and expansion test results
[0086]
[0087]
[0088] It can be seen from Table 3 that compared with the early-strength polycarboxylate water-reducing agent of Comparative Examples 1 to 3, the low-temperature early-strength water-reducing agent prepared according to Examples 1 to 3 can significantly increase the slump and expansion of concrete, improve the flowability of concrete, and after 0.5h and 1h of time loss, the slump and expansion retention performance of the concrete synthesized by the low-temperature early-strength water-reducing agent of Examples 1 to 3 is significantly better than the slump and expansion retention performance of the concrete mixed with the early-strength polycarboxylate water-reducing agent of Comparative Examples 1 to 3.
[0089] (2) Compressive strength of concrete at different curing temperatures:
[0090] In order to investigate the effect of the low-temperature early-strength water-reducing agent synthesized by the present invention on the early strength development of concrete under low temperature and negative temperature environment, the proportions of the various components of the concrete were controlled to be the same, and concrete specimens were formed according to GB / T 50081. The surface was immediately covered with a waterproof film after mold filling, and then placed at -10--5°C, -5-0°C and 0-5°C for curing for 24h, respectively. After demolding, the compressive strength of the concrete specimens was tested at 1d, and the remaining concrete specimens continued to be placed at -10--5°C, -5-0°C and 0-5°C for curing to the specified age, and the compressive strength of the concrete specimens at 3d and 28d were tested, respectively. The test results are shown in Table 4.
[0091] Table 4 Concrete compressive strength test results (MPa)
[0092]
[0093]
[0094] It can be seen from Table 4 that at different curing temperatures, the compressive strength of the concrete specimens mixed with the low-temperature and early-strength polycarboxylate water-reducing agent prepared in Examples 1 to 3 at different curing ages is significantly higher than the compressive strength of the concrete specimens mixed with the early-strength polycarboxylate water-reducing agent in Comparative Examples 1 to 3, and the early strength and late strength of the concrete specimens are significantly improved, indicating that the low-temperature and early-strength water-reducing agent prepared in the present invention can promote the development of the early strength of concrete under low temperature and negative temperature curing environments.
[0095] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A low-temperature early-strength water reducer, characterized in that: The structural formula of the low-temperature early-strength water reducer is as follows: Among them, the structural formula of R' is: Among them, the wavy line position is the connection position, R is CH2, CH2CH2 or O(CH2CH2O)2, R1 is H, CH3, CH2CH3 or CH2COOH, R2 is H or CH3, R3 is H, OH, CH3O, Cl or Br, R4 is H, OH, CH3O or Cl, and R5 is H or Na; a, b, c, d, m, n, x and f are integers, indicating the number of repeating units of each part in the polymer, a is 10 to 150, b is 3 to 40, c is 3 to 30, d is 3 to 50, m is 0 to 100, n is 10 to 150, x is 2 to 10, and f is 1 to 5.
2. The method for preparing the low-temperature early-strength water reducing agent according to claim 1, characterized in that: The steps include: (1) dissolving chitosan in solvent 1 to obtain mixed solution 1; activating unsaturated carboxylic acid small monomer, solvent 2 and activator to obtain mixed solution 2; adding mixed solution 2 to mixed solution 1 to carry out amidation reaction, and then dialyzing and vacuum drying in sequence to obtain amidated product 1; (2) reacting poly(ethylene glycol) methacrylate, bipyridine and solvent 3 to obtain a mixed solution 3; mixing N,N'-disuccinimidyl carbonate, a pyridine compound and solvent 4 and adding the mixture to the mixed solution 3 to carry out an esterification reaction, and then successively performing reduced pressure distillation and purification to obtain an esterification product; (3) reacting the amidation product 1 with the solvent 1 to obtain a mixed solution 4; dissolving the esterification product in the solvent 5 and then dropwise adding the mixture to the mixed solution 4 to perform a Michael addition reaction, followed by dialysis and vacuum drying to obtain a Michael addition product; (4) mixing the polyether macromonomer and the solvent 5 to obtain a bottom liquid, first adding an oxidant to the bottom liquid and stirring it evenly, and then simultaneously dropping liquid A, liquid B and liquid C into the bottom liquid; wherein liquid A is a mixture of an olefinic acid small monomer, a sulfonic acid small monomer and the solvent 5, liquid B is a mixture of a Michael addition product and the solvent 5, and liquid C is a mixture of a reducing agent, a chain transfer agent and the solvent 5; after the dropwise addition is completed, performing a free radical polymerization reaction, and performing reduced pressure distillation to obtain a free radical polymerization product; (5) subjecting the free radical polymerization product, the catalyst, the solvent 6 and the alkaline solution to a Hofmann degradation reaction, followed by purification and vacuum drying to obtain a Hofmann degradation product; (6) reacting the Hofmann degradation product with solvent 5 to obtain a mixed solution 6; dissolving the anhydride small monomer in solvent 7 and heating it in a water bath to obtain a mixed solution 7; subjecting the mixed solution 6, the mixed solution 7 and the amine small monomer to an amidation reaction, followed by dialysis and vacuum drying to obtain an amidated product 2; (7) Trehalose, triphenylphosphine and solvent 4 are mixed, and an amine compound is added dropwise thereto to carry out reaction 1. After reaction 1 is completed, an ester substance and an alcohol substance are added thereto in sequence to carry out reaction 2, followed by extraction, washing and vacuum drying to obtain thiolated trehalose; amidation product 2 is reacted with solvent 4 to obtain a mixed solution 8; thiolated trehalose is dissolved in solvent 2, and solvent 8 is added to mix well, and the mixed solution is added to the mixed solution 8 to carry out a Thiol-ene reaction, and then the mixture is cooled to room temperature and purified in sequence to obtain a low-temperature early-strength water reducer.
3. The method for preparing the low-temperature early-strength water reducing agent according to claim 2, characterized in that: In the step (1), solvent 1 includes acetic acid or hydrochloric acid, and the mass concentration of solvent 1 is 0.5-2%; the unsaturated carboxylic acid small monomer includes cinnamic acid, m-chlorocinnamic acid, m-bromocinnamic acid, p-chlorocinnamic acid, p-bromocinnamic acid, caffeic acid or 3,4-dimethoxycinnamic acid; solvent 2 includes phosphate buffer; the activator includes 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide The molar ratio of amine is 1-2:1; the molar ratio of chitosan and unsaturated carboxylic acid small monomer is 1-2:1; the molar ratio of activator and unsaturated carboxylic acid small monomer is 2-4:1; the mass ratio of solvent 1, solvent 2 and chitosan is 40-60:20-40:1; the dissolution temperature is 20-30°C, and the dissolution time is 12-24h; the activation temperature is 20-30°C, and the activation time is 1-3h; the amidation reaction temperature is 30-35°C, and the amidation reaction time is 2-6h.
4. The method for preparing the low-temperature early-strength water reducing agent according to claim 2 or 3, characterized in that: In the step (2), solvent 3 includes water or anhydrous ethanol; the pyridine compound includes pyridine, 4-dimethylaminopyridine or 2-bromo-4-dimethylaminopyridine; solvent 4 includes one or more of N,N-dimethylformamide, N,4-dimethylformamide and dimethyl sulfoxide; the molar ratio of poly(ethylene glycol) methacrylate, bipyridine, N,N'-disuccinimidyl carbonate and pyridine compound is 10-40:1:30-60:40-60; the mass ratio of poly(ethylene glycol) methacrylate, solvent 3 and solvent 4 is 1:30-60:40-80; the reaction is carried out under nitrogen conditions, and the reaction time is 10-30 minutes; the esterification reaction is carried out under nitrogen conditions, the esterification reaction temperature is 70-90°C, and the esterification reaction time is 4-6 hours.
5. The method for preparing the low-temperature early-strength water reducing agent according to claim 4, characterized in that: In the step (3), solvent 1 includes acetic acid or hydrochloric acid, and the mass concentration of solvent 1 is 0.5-2%; solvent 5 is water; the molar ratio of esterification product and amidation product 1 is 0.5-1:1; the mass ratio of amidation product 1, solvent 1 and solvent 5 is 1:60-120:40-80; the reaction is carried out under nitrogen conditions, the reaction temperature is 30-50°C, and the reaction time is 1-3h; the dropwise addition time is 40-80min; the Michael addition reaction is carried out under nitrogen conditions, the Michael addition reaction temperature is 50-70°C, and the Michael addition reaction time is 20-24h.
6. The method for preparing the low-temperature early-strength water reducing agent according to claim 5, characterized in that: In the step (4), the polyether macromonomer includes methyl allyl polyoxyethylene ether, isopentanol polyethoxyethylene ether or butanediol monovinyl polyoxyethylene ether, and the molecular weight of the polyether macromonomer is 2000-5000 g / mol; the solvent 5 independently includes water; the oxidant includes H2O2, ammonium persulfate, potassium persulfate or sodium persulfate; the olefinic acid small monomer includes acrylic acid, methacrylic acid, 2-ethylacrylic acid, maleic anhydride, itaconic acid, crotonic acid, crotonic anhydride, isomethacrylic acid or trans-2-pentenoic acid; the sulfonic acid small monomer includes 2-acrylamide-2-methylpropanesulfonic acid or 2-methyl-2-[(1-oxo-2-propenyl)amino]-1-propanesulfonic acid sodium salt; the reducing agent includes one or more of ascorbic acid, bleaching powder and FeSO4; the chain transfer agent includes thioglycolic acid, 3-mercaptopropionic acid, sodium hypophosphite, sodium allylpropanesulfonate or sodium methacrylic acid; The molar ratio of the polyether macromonomer and the olefinic acid small monomer is 1:4-8; the molar ratio of the oxidant, the olefinic acid small monomer, the sulfonic acid small monomer, the Michael addition product, the reducing agent and the chain transfer agent is 0.03-0.1:1:0.035-0.1:0.035-0.1:0.003-0.01:0.01-0.2; during the mixing process of the polyether macromonomer and the solvent 5, the mass ratio of the polyether macromonomer and the solvent 5 is 1:20-160; the ratio of the total mass of the olefinic acid small monomer and the sulfonic acid small monomer in liquid A to the mass of the solvent 5 is 1:10-40; the mass ratio of the Michael addition product to the solvent 5 in liquid B is 1:10-20; the ratio of the total mass of the reducing agent and the chain transfer agent in liquid C to the mass of the solvent 5 is 1:10-20; the time of the dropwise addition is 40-80 min; the temperature of the free radical polymerization reaction is 20-70° C., and the time of the free radical polymerization reaction is 2-6 h.
7. The method for preparing the low-temperature early-strength water reducing agent according to claim 6, characterized in that: In the step (5), the catalyst includes one or more of silver chloride, cuprous bromide, bromine, sodium chlorite, and sodium bromite; the solvent 6 includes anhydrous ethanol or water; the alkaline solution includes one or more of NaOH aqueous solution, KOH aqueous solution, and NH4OH aqueous solution, and the mass concentration of the alkaline solution is 4-6%; the molar ratio of the free radical polymerization product and the catalyst is 10-20:1; the mass ratio of the free radical polymerization product, the solvent 6, and the alkaline solution is 1:30-100:20-40; the Hofmann degradation reaction includes a first-stage Hofmann degradation reaction and a second-stage Hofmann degradation reaction; the parameters of the first-stage Hofmann degradation reaction are as follows: argon gas conditions, a temperature of 20-30°C, and a time of 30-50 min; the parameters of the second-stage Hofmann degradation reaction are as follows: argon gas conditions, a temperature of 120-180°C, and a time of 4-8 h.
8. The method for preparing the low-temperature early-strength water reducing agent according to claim 6 or 7, characterized in that: In the step (6), the solvent 5 is water; the anhydride small monomer includes nadic anhydride or cis-5-naphthene-exo-2,3-dicarboxylic anhydride; the solvent 7 includes one or more of tetrahydrofuran, benzene, toluene, methanol, ethanol, isopropanol, and n-butanol, and the mass concentration of the solvent 7 is 4-6%; the amine small monomer includes ethylenediamine, tetramethylenediamine, 1,4-butanediamine, 1,6-hexanediamine, 1,8-octanediamine or decanediamine; the Hofmann degradation product and the anhydride small monomer include nadic anhydride or cis-5-naphthene-exo-2,3-dicarboxylic anhydride; the solvent 7 includes one or more of tetrahydrofuran, benzene, toluene, methanol, ethanol, isopropanol, and n-butanol, and the mass concentration of the solvent 7 is 4-6%. The molar ratio of the monomers is 1-4:1; the molar ratio of the Hofmann degradation product, the solvent 7 and the amine small monomer is 1:1-2:1-2; the mass ratio of the Hofmann degradation product and the solvent 5 is 1:40-60; the reaction temperature is 20-30°C, and the reaction time is 4-8h; the water bath heating temperature is 40-60°C, and the water bath heating time is 0.5-1h; the amidation reaction temperature is 20-30°C, and the amidation reaction time is 12-24h.
9. The method for preparing the low-temperature early-strength water reducing agent according to claim 8, characterized in that: In the step (7), the solvent 4 independently includes one or more of N,N-dimethylformamide, N,4-dimethylformamide, and dimethyl sulfoxide; the amine compound includes N-bromosuccinimide and / or N-hydroxysuccinimide; the ester substance includes ethyl acetate, ethyl propionate, ethyl butyrate, ethyl isobutyrate, ethyl valerate or ethyl isovalerate; the alcohol substance includes DL-dithiothreitol, dithiothreitol, dithioerythritol, L-1,4-dithiothreitol, 1,2-butanethiol, 1,4-butanethiol, 2,3-butanethiol, 1,6-hexanethiol, 1,2-ethanedithiol or 1,5-pentanedithiol; solvent 2 includes phosphate buffer; solvent 8 includes one or more of 240-260 mg / ml methanol, 0.01-0.03 w / v% eosin, and 0.1-0.3 v / v% triethanolamine; the molar ratio of trehalose to triphenylphosphine is 0.2-0.8:1; the molar ratio of trehalose to alcohol substances is 1:2-4; the molar ratio of triphenylphosphine, amine compounds and ester substances is 1:1-2:1-3; the molar ratio of amidation product 2 to thiolated trehalose is 2-4:1; solvent 2, solvent 8 and thiol The mass ratio of trehalose to triphenylphosphine is 20-40:5-20:1; during the mixing process of trehalose, triphenylphosphine and solvent 4, the mass ratio of solvent 4 to trehalose is 30-60:1; in the mixed solution 8, the mass ratio of solvent 4 to amidation product 2 is 10-40:1; the time of dropwise addition is 1-2h; the temperature of reaction 1 is 20-30°C, and the time of reaction 1 is 36-48h; the temperature of reaction 2 is 20-30°C, and the time of reaction 2 is 12-24h; the temperature of the reaction is 20-30°C, and the time of the reaction is 12-24h; the Thiol-ene reaction includes the reaction of The reaction material is subjected to the first-stage Thiol-ene reaction, the pH value is adjusted, and the second-stage Thiol-ene reaction is performed in sequence; the parameters of the first-stage Thiol-ene reaction are as follows: nitrogen conditions, ultraviolet light irradiation, a temperature of 20 to 30°C, and a time of 12 to 24 hours; the pH adjuster used for adjusting the pH value includes one or more of phosphate buffer, oxalic acid, acetic acid, and citric acid, and the pH value is adjusted to 6 to 8; the parameters of the second-stage Thiol-ene reaction are as follows: nitrogen conditions, ultraviolet light irradiation, a temperature of 30 to 40°C, and a time of 10 to 30 minutes.
10. The method for preparing the low-temperature early-strength water reducing agent according to claim 9, characterized in that: In the steps (1) to (7), the dialysis is independently performed using a dialysis bag, and the dialysis time is independently 48 to 72 hours; the vacuum drying time is independently 24 to 48 hours; the temperature of the reduced pressure distillation is independently 100 to 115° C.; the extraction agent used for the extraction includes one or more of benzene, toluene, xylene, and chloroform; and the cleaning reagent includes anhydrous ethanol.
Citation Information
Patent Citations
Ethers early strength type polycarboxylate water reducer and preparation method thereof
CN103450408A
Preparation method of triisopropanolamine modified early strength polycarboxylate superplasticizer
CN103936934A
Early strength type polycarboxylate superplasticizer as well as preparation method and application thereof
CN107151294A
Slump-retaining early-strength functional monomer, slump-retaining early-strength polycarboxylate superplasticizer and preparation method of slump-retaining early-strength functional monomer
CN114478962A
Composite early-strength polycarboxylate superplasticizer and preparation method thereof
CN116535134A
Cited By
Polycarboxylate superplasticizer as well as preparation method and application thereof
CN119823329A
Mine supporting material interface reinforcing agent, its preparation method and application
CN122916503A