Length-controllable polyfluorene polythiophene segmented copolymer nanowire and preparation method thereof

The polyfluorene polythiophene conjugated polymer was synthesized through a nickel complex catalyst and annealed treatment, which solved the problem of nanowire length control, achieved length consistency of nanowire preparation, and improved its physical, chemical and mechanical properties.

CN118955876AActive Publication Date: 2024-11-15HUAIBEI NORMAL UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411027725.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The prior art is difficult to accurately control the length of nanowires, which affects the performance of their physical, chemical and mechanical properties, and the control of the self-assembly process is difficult.

Method used

The polyfluorene polythiophene conjugated polymer was synthesized by transfer polymerization of the active catalyst by using nickel complex as a catalyst, and annealed treatment was used to form a polyfluorene polythiophene block copolymer nanowire with controllable length.

Benefits of technology

Accurate control of the length of nanowires is achieved, which significantly affects its physical, chemical and mechanical properties, ensures the consistency and narrow dispersion of nanowires, and improves the predictability of their performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955876A_ABST
    Figure CN118955876A_ABST
Patent Text Reader

Abstract

The invention discloses a length-controllable polyfluorene polythiophene segmented copolymer nanowire and a preparation method thereof. The structural formula of a polyfluorene polythiophene segmented copolymer is shown in the specification. The polyfluorene polythiophene segmented copolymer nanowire of which the length is gradually increased along with the increase of the annealing temperature is obtained after the segmented copolymer is subjected to annealing treatment; according to the method disclosed by the invention, crystal self-assembly can be realized, the nanowire with controllable length and narrow dispersity is prepared, and the length and consistency of the nanowire are accurately controlled; the physical, chemical and mechanical properties of the nanowire can be optimized by accurately controlling the length and consistency of the nanowire, so that the nanowire with controllable length and narrow dispersibility can ensure the consistency and predictability of the performance exerted by the nanowire.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high molecular polymer nanowire preparation, and specifically relates to a polyfluorene-polythiophene block copolymer nanowire with controllable length and a preparation method thereof Background Art

[0002] The progress of supramolecular chemistry provides an excellent platform for creating and constructing a wide range of synthetic configurations, from molecular machines at the molecular scale to one-dimensional or two-dimensional nanostructures of supramolecular polymers, and even materials at the macroscopic level. At the same time, the size and shape of supramolecular polymers can be controlled by monomer selection, chain structure design, and changes in solvent conditions (such as solvent mixtures, pH manipulation, salt concentration, and temperature).

[0003] Amphiphilic block copolymers containing conjugated polymer core-forming blocks are usually assembled in solution to form micelles, however, precise control of the self-assembly process remains a challenge. Active crystallization-driven self-assembly is an efficient seed growth strategy for the preparation of morphologically pure, low-dispersity one-dimensional fibers and two-dimensional platelets to achieve size control. In addition, for nanowire materials, precise control of the length of the nanowires plays an important role in the physical, chemical and mechanical properties of the nanowire materials. In addition, how to control the consistency of the length of the nanowires is also a major technical challenge in this field.

[0004] The present invention aims to develop a new nanowire preparation process to solve the above-mentioned technical challenges in the field. Summary of the invention

[0005] The present invention uses nickel complex as catalyst, adopts active catalyst transfer polymerization method, and synthesizes polyfluorene polythiophene conjugated polymer by one-pot method. By utilizing the crystallization property of polyfluorene, crystallization drives self-assembly, and nanowires with controllable length and narrow dispersion can be formed.

[0006] In one aspect, the present invention provides a length-controllable polyfluorene-polythiophene block copolymer nanowire, wherein the structural formula of the polyfluorene-polythiophene block copolymer is as follows: Wherein m and n are positive integers that make the number average molecular weight of the block copolymer pair between 10,000 and 50,000; after annealing, the block copolymer obtains a polyfluorene-polythiophene block copolymer nanowire whose length gradually increases with the increase of annealing temperature. The precise control of the length of the nanowire by the annealing temperature is of great significance for the preparation of the nanowire, and the length of the nanowire can significantly affect its physical, chemical and mechanical properties. Therefore, the prepared length-controllable polymer nanowire of the present invention substantially realizes the precise control of the physical and chemical properties of the nanowire.

[0007] Preferably, the annealing temperature ranges from 35 to 60° C. The annealing temperature range is relatively low, which reduces the difficulty of control.

[0008] Preferably, the length of the polyfluorene-polythiophene block copolymer nanowire is 60-2000 nm. It is easy to understand that any length in this range can be achieved, such as 70 nm, 80 nm, 100 nm, 200 nm, 500 nm, 1000 nm, 1500 nm, etc.

[0009] Preferably, the polydispersity coefficient of the polyfluorene polythiophene block copolymer nanowire is Lw / Ln of 1.01-1.04, where Lw represents the weight average contour length and Ln represents the number average contour length. The polydispersity coefficient of the nanowire is close to 1, indicating that the consistency of the assembly is very high, so that the nanowires with consistent lengths are finally obtained, which is of great significance for the further development and utilization of the nanowires. In addition, the molecular weight distribution of the polyfluorene polythiophene block copolymer is 1.1-1.3, that is, the molecular weight distribution of the synthesized polymer is also relatively narrow, which lays the foundation for the subsequent synthesis of nanowires with high consistency.

[0010] On the other hand, the present invention provides a method for preparing polyfluorene-polythiophene block copolymer nanowires, comprising the following steps:

[0011] S1. Prepare a polyfluorene-polythiophene block copolymer, the structural formula of which is shown below:

[0012] Wherein m and n are positive integers such that the number average molecular weight of the block copolymer pair is between 10,000 and 50,000.

[0013] S2, dissolving the polyfluorene-polythiophene block copolymer in tetrahydrofuran solvent.

[0014] S3, dripping the tetrahydrofuran solution containing the polyfluorene-polythiophene block copolymer dissolved in step S2 into the mixed solvent and letting it stand for a period of time to obtain a polyfluorene-polythiophene block copolymer nanowire seed precursor solution.

[0015] S4. Ultrasonic treatment is performed on the nanowire seed precursor solution in step S3 to obtain a polyfluorene-polythiophene block copolymer nanowire seed solution.

[0016] S5. Annealing the nanowire seed solution in step S4 at 35-60°C, and then standing at 25°C for a period of time to obtain polyfluorene-polythiophene block copolymer nanowires with controllable length.

[0017] Preferably, the mixed solvent is composed of chloroform and methanol, and the volume ratio of chloroform to methanol is 1: 1. The selection of the mixed solution and the selection of the ratio are of great significance for the preparation of nanowires. It is found through experiments that a chloroform / methanol mixed solvent with a volume ratio of 1: 1 is very critical for the preparation of nanowire seed precursor solution.

[0018] Preferably, the annealing time in step 5 is 0.5-2 hours, and the standing time in steps S3 and S5 is 2-4 days.

[0019] Preferably, the ultrasonic treatment in step S4 is performed at 0° C. for 0.5 hours.

[0020] Preferably, the preparation method of the polyfluorene-polythiophene block copolymer in step S1 is as follows, wherein C6H 13 is n-hexyl, and comprises the following steps:

[0021] T1. Add fluorene monomer, lithium chloride and isopropyl magnesium chloride into a reaction container, wherein the structural formula of the fluorene monomer is shown below; evacuate the reaction container and fill it with nitrogen to atmospheric pressure; add tetrahydrofuran solvent and react at -20°C for a period of time; add nickel complex Ni(acac)2 / dppp and react at 0°C for a period of time to obtain a solution containing a polyfluorene polymer.

[0022] T2, adding thiophene monomer and isopropyl magnesium chloride to another reaction container, evacuating the reaction container and filling it with nitrogen to atmospheric pressure, adding tetrahydrofuran solvent, and reacting at room temperature for a period of time to obtain the thiophene structure shown below; then adding the solution containing the polyfluorene polymer in step T1, reacting at room temperature for a period of time, and obtaining the polyfluorene-polythiophene block copolymer after post-treatment.

[0023]

[0024] Preferably, the post-treatment operation in step T2 is to add ether to the reaction solution to terminate the reaction, wash the obtained product with ether for 4-5 times, and vacuum dry until the mass remains unchanged.

[0025] Nickel complex Ni(acac)2 / dppp is a commonly used catalyst in the field of polymer synthesis. The synthesis method of the nickel complex catalyst Ni(acac)2 / dppp adopted in the present invention comprises the following steps: taking a 25mL polymerization bottle, weighing 51.4mg of nickel acetylacetonate, 84.1mg of 1,3-bis(diphenylphosphine)propane (ligand=dppp, Ni(acac)2 / dppp=1 / 1.02), adding 10mL of tetrahydrofuran under a nitrogen atmosphere, and stirring at room temperature.

[0026] Compared with the prior art, the technical solution provided by the present invention exhibits the following beneficial effects.

[0027] The present invention provides a length-controllable polyfluorene-polythiophene block copolymer nanowire, which can achieve precise control of the nanowire in the length range of 60-1000nm by adjusting the nanowire annealing problem. In addition, the polydispersity coefficient of the prepared nanowire is 1.01-1.04, that is, the prepared nanowire has a narrow dispersity and a high degree of consistency. Therefore, the technical solution provided by the present invention can be used to prepare nanowires with controllable length and narrow dispersity. By precisely controlling the length and consistency of the nanowire, its physical, chemical and mechanical properties can be optimized, so the nanowire with controllable length and narrow dispersity can ensure the consistency and predictability of its performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is the gel permeation chromatogram of each polymer involved in Examples 1-5.

[0029] Figure 2 is the hydrogen spectrum of the copolymer prepared in Example 1.

[0030] Figure 3 It is the SEM picture of the copolymer nanowire seeds prepared in Example 6 under different proportions of mixed solvents.

[0031] Figure 4 These are SEM images of copolymer nanowire seeds and copolymer nanowires obtained after treatment at different annealing temperatures. DETAILED DESCRIPTION

[0032] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following will briefly introduce the drawings required for use in the specific embodiments or the prior art description. Obviously, the drawings in the following description are some embodiments of the present invention. For ordinary technicians in this field, other drawings can also be obtained based on these drawings without paying creative work. The present invention has many different forms of implementation and should not be understood as being limited to the embodiments described herein. On the contrary, these embodiments are provided so that the present disclosure will be thorough and complete, and the concept of the present invention will be fully conveyed to those skilled in the art. The present invention will only be limited by the claims.

[0033] The synthesis method of the nickel complex catalyst used in the present invention comprises the following steps: taking a 25 mL polymerization bottle, weighing 51.4 mg of nickel acetylacetonate, 84.1 mg of 1,3-bis(diphenylphosphine)propane (ligand = dppp, Ni(acac)2 / dppp = 1 / 1.02), adding 10 mL of tetrahydrofuran under a nitrogen atmosphere, and stirring at room temperature.

[0034] Example 1

[0035] The synthesis route of the polyfluorene-polythiophene block copolymer of the present invention is shown in the figure below. The specific preparation process is as follows: 269 mg (0.5 mmol) of fluorene monomer is added to a 50 mL polymerization bottle. The specific structure of the fluorene monomer is shown in the figure, and the -C6H 13 represents n-hexyl, 42.4 mg lithium chloride, and then 0.25 ml isopropyl magnesium chloride are added, and the polymerization bottle is vacuumed and filled with nitrogen, which is repeated 3 times, and then 10 mL dry tetrahydrofuran is added, and the reaction is carried out at -20°C for 2 hours; under a nitrogen environment, 1 mL of nickel complex catalyst solution is added, wherein the ratio of fluorene monomer to nickel complex catalyst is 25:1, and the reaction is carried out at 0°C for 2 hours, so as to obtain a polyfluorene polymer. See the attached Figure 1 As shown in the figure, the polyfluorene polymer described in this embodiment is poly-1 25 The number average molecular weight of the polyfluorene polymer was 7.68×10 3 , the molecular weight distribution is 1.27.

[0036] 23 mg of hydrophilic thiophene monomer was placed in a 10 mL polymerization bottle. The polymerization bottle was evacuated and filled with nitrogen for 3 times. 1 mL of dry tetrahydrofuran was added, followed by 0.1 mL of isopropyl magnesium chloride. The reaction was continued at room temperature for 1 hour. 1 mL of the polymer solution in the previous step was added, and the reaction was continued at room temperature for 2 hours. Ether was added to terminate the reaction. The obtained product was washed with ether for 4-5 times and vacuum dried until the mass remained unchanged. The polyfluorene-polythiophene polymer was obtained, with a mass of 43.1 mg. See attached. Figure 1 As shown in the figure, the polyfluorene-polythiophene copolymer described in this embodiment is poly(1 25 -b-2 25 ), and the number average molecular weight of the polyfluorene polymer was 15.8×10 3 , molecular weight distribution is 1.25. In addition, see Appendix Figure 2 This is the hydrogen spectrum of the prepared copolymer. The figure clearly shows the distribution of hydrogen elements in multiple locations in the copolymer structure, indicating that a copolymer shown in the following structural formula was prepared.

[0037]

[0038] Embodiment 2,

[0039] The experimental steps are the same as those in Example 1, except that 9.2 mg of hydrophilic thiophene monomer and 0.04 ml of isopropyl magnesium chloride are added, and the mass of the polyfluorene-polythiophene polymer finally prepared is 31.2 mg.

[0040] See attached Figure 1 As shown in the figure, the polyfluorene-polythiophene copolymer described in this embodiment is poly(1 25 -b-210 ), and the number average molecular weight of the polyfluorene-polythiophene copolymer was 10.38×10 3 , the molecular weight distribution is 1.23.

[0041] Example 3

[0042] The experimental steps are the same as those in Example 1, except that 27.6 mg of hydrophilic thiophene monomer and 0.12 ml of isopropyl magnesium chloride are added, and the mass of the polyfluorene-polythiophene polymer finally prepared is 47.2 mg.

[0043] See attached Figure 1 As shown in the figure, the polyfluorene-polythiophene copolymer described in this embodiment is poly(1 25 -b-2 30 ), and the number average molecular weight of the polyfluorene-polythiophene copolymer was 19.63×10 3 , the molecular weight distribution is 1.13.

[0044] Example 4

[0045] The experimental steps are the same as those in Example 1, except that 64.4 mg of hydrophilic thiophene monomer and 0.28 ml of isopropyl magnesium chloride are added, and the mass of the polyfluorene-polythiophene polymer finally prepared is 82.8 mg.

[0046] See attached Figure 1 As shown in the figure, the polyfluorene-polythiophene copolymer described in this embodiment is poly(1 25 -b-2 70 ), and the number average molecular weight of the polyfluorene-polythiophene copolymer was 28.49×10 3 , the molecular weight distribution is 1.13.

[0047] Example 5

[0048] The experimental steps are the same as those in Example 1, except that 73.6 mg of hydrophilic thiophene monomer and 0.31 ml of isopropyl magnesium chloride are added, and the mass of the polyfluorene-polythiophene polymer finally prepared is 90.6 mg.

[0049] See attached Figure 1 As shown in the figure, the polyfluorene-polythiophene copolymer described in this embodiment is poly(1 25 -b-2 80 ), the number average molecular weight of the polyfluorene-polythiophene copolymer was 35.45×10 3 , the molecular weight distribution is 1.12.

[0050] Example 6

[0051] The experimental steps are the same as those in Example 1, except that 110.4 mg of hydrophilic thiophene monomer and 0.48 ml of isopropyl magnesium chloride are added, and the mass of the polyfluorene-polythiophene polymer finally prepared is 116.7 mg.

[0052] See attached Figure 1 As shown in the figure, the polyfluorene-polythiophene copolymer described in this embodiment is poly(1 25 -b-2 120 ), the number average molecular weight of the polyfluorene-polythiophene copolymer was 47.46×10 3 , the molecular weight distribution is 1.14.

[0053] Figure 1 The polyfluorene polymer and the polyfluorene-polythiophene polymer prepared in Examples 1-7 are shown together, and their gel chromatograms are arranged from right to left.

[0054] Embodiment 7,

[0055] Take 60 mg of the polyfluorene-polythiophene copolymer prepared in Example 1 and dissolve it in 10 mL of tetrahydrofuran to obtain a copolymer solution. Take 30 uL of the above copolymer solution and drop it into a culture bottle containing 1 mL of a chloroform / methanol mixed solvent. Then cover the mouth of the culture bottle with a rubber diaphragm and detect it with a SEM after standing for 3 days. The volume ratio of chloroform to methanol is set to 10:0, 9:1, 8:2, 7:3, 6:4, 5:5, 4:6, 3:7, 2:8, 1:9, and 0:10, respectively. Among them, 10:0 means that the solvent used is pure chloroform solvent, and 0:10 means that the solvent used is pure methanol solvent. See Appendix Figure 3 It is known that Figure 3 The copolymer nanowire seed precursors obtained under the above 11 solvent conditions are shown in a top-to-bottom and left-to-right order. It can be seen that when pure chloroform solvent is used, no assembly is found; when the ratio of chloroform / methanol in the solvent is set to 9:1 and 8:2, some less obvious assembly situations can be found; when the ratio of chloroform / methanol in the solvent is set to 7:3 and 6:4, some self-assembly phenomena can be found, but the assembly morphology is an irregular nanosphere morphology structure; when the ratio of chloroform / methanol in the solvent is set to 5:5, an obvious long strip nanowire structure is formed, and the width is uniform, which is an ideal nanowire seed precursor; when the ratio of chloroform / methanol in the solvent is set to 4:6, the nanowire structure is not obvious, and a small amount of nanosphere structure appears; when the ratio of chloroform / methanol in the solvent is set to 3:7, 2:8, 1:9 and 0:10, nanosphere morphology structures appear. In summary, when the ratio of chloroform / methanol in the solvent is set to 5:5, it can be seen that a well-structured copolymer nanoseed precursor solution is prepared.

[0056] Example 8

[0057] The nanoseed precursor solution of Example 7 was subjected to ultrasonic treatment at 0°C for 0.5 h to obtain a polyfluorene-polythiophene block copolymer nanowire seed solution. Figure 4 It can be seen that the nanometer length of the prepared seeds is 82nm, and the polydispersity coefficient Lw / Ln is 1.04. Take 1mL of the equivalent batch of the polyfluorene polythiophene block copolymer nanowire seed solution obtained above and transfer it to 6 culture bottles and cover them with rubber diaphragms. These culture bottles are placed in oil baths at different temperatures for annealing for 1 hour. The temperature of the oil bath is controlled at 35, 40, 45, 55 and 60°C respectively. After the annealing treatment is completed, the culture bottles are transferred to a 25°C oil bath and placed for 3 days. Then, the samples in each culture bottle are subjected to SEM detection. It can be clearly seen that when the annealing temperature is 35°C, the copolymer nanowires obtained are 340nm, and the polydispersity coefficient Lw / Ln is 1.03; when the annealing temperature is 40°C, the copolymer nanowires obtained are 520nm, and the polydispersity coefficient Lw / Ln is 1.03; when the annealing temperature is 45°C, the copolymer nanowires obtained are 640nm, and the polydispersity coefficient Lw / Ln is 1.01; when the annealing temperature is 55°C, the copolymer nanowires obtained are 1500nm, and the polydispersity coefficient Lw / Ln is 1.04; when the annealing temperature is 60°C, the copolymer nanowires obtained are 1900nm, and the polydispersity coefficient Lw / Ln is 1.05. It can be seen that after the block copolymer is annealed, the polyfluorene-polythiophene block copolymer nanowires whose length gradually increases with the increase of the annealing temperature are obtained. Moreover, the polydispersity coefficient Lw / Ln of these nanowires is close to 1 and the dispersion is narrow, indicating good consistency, which is of great significance for the subsequent physical, chemical and / or mechanical properties of the nanowires in functional materials.

[0058] The present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A length-controllable polyfluorene-polythiophene block copolymer nanowire, characterized in that: The structural formula of the polyfluorene-polythiophene block copolymer is as follows: Wherein m and n are positive integers such that the number average molecular weight of the block copolymer pair is between 10,000 and 50,000; After the block copolymer is annealed, a polyfluorene-polythiophene block copolymer nanowire is obtained, the length of which gradually increases as the annealing temperature rises.

2. The polyfluorene-polythiophene block copolymer nanowire according to claim 1, characterized in that: The annealing temperature ranges from 35 to 60°C.

3. The polyfluorene-polythiophene block copolymer nanowire according to claim 1, characterized in that: The length of the polyfluorene-polythiophene block copolymer nanowire is 70-2000nm.

4. The polyfluorene-polythiophene block copolymer nanowire according to claim 1, characterized in that: The polydispersity coefficient Lw / Ln of the polyfluorene-polythiophene block copolymer nanowire is 1.01-1.04, wherein Lw represents the weight average contour length and Ln represents the number average contour length; the molecular weight distribution of the polyfluorene-polythiophene block copolymer is 1.1-1.

3.

5. The method for preparing polyfluorene-polythiophene block copolymer nanowires according to claims 1-4, comprising the following steps: S1. Prepare a polyfluorene-polythiophene block copolymer, the structural formula of which is shown below: Wherein m and n are positive integers such that the number average molecular weight of the block copolymer pair is between 10,000 and 50,000; S2, dissolving the polyfluorene-polythiophene block copolymer in tetrahydrofuran solvent; S3, dropping the tetrahydrofuran solution containing the polyfluorene-polythiophene block copolymer dissolved in step S2 into the mixed solvent and letting it stand for a period of time to obtain a polyfluorene-polythiophene block copolymer nanowire seed precursor solution; S4, ultrasonically treating the nanowire seed precursor solution in step S3 to obtain a polyfluorene-polythiophene block copolymer nanowire seed solution; S5. Annealing the nanowire seed solution in step S4 at 35-60° C., and then standing at 25° C. for a period of time to obtain polyfluorene-polythiophene block copolymer nanowires with controllable length.

6. The method for preparing polyfluorene-polythiophene block copolymer nanowires according to claim 5, characterized in that: The mixed solvent consists of chloroform and methanol, and the volume ratio of chloroform to methanol is 1:

1.

7. The method for preparing polyfluorene-polythiophene block copolymer nanowires according to claim 5, characterized in that: The annealing time in step 5 is 0.5-2 hours, and the standing time in steps S3 and S5 is 2-4 days.

8. The method for preparing polyfluorene-polythiophene block copolymer nanowires according to claim 5, characterized in that: The ultrasonic treatment in step S4 was performed at 0°C for 0.5 hours.

9. The method for preparing polyfluorene-polythiophene block copolymer nanowires according to claim 5, characterized in that: The preparation method of the polyfluorene-polythiophene block copolymer in step S1 is as follows, wherein C6H 13 is n-hexyl, and comprises the following steps: T1, adding fluorene monomer, lithium chloride and isopropyl magnesium chloride into a reaction container, wherein the fluorene monomer has a structural formula as shown below, evacuating the reaction container and filling it with nitrogen to atmospheric pressure, adding tetrahydrofuran solvent, reacting at -20°C for a period of time, adding nickel complex catalyst Ni(acac)2 / dppp, reacting at 0°C for a period of time, and obtaining a solution containing a polyfluorene polymer; T2, adding thiophene monomer and isopropyl magnesium chloride to another reaction container, evacuating the reaction container and filling it with nitrogen to atmospheric pressure, adding tetrahydrofuran solvent, reacting at room temperature for a period of time to obtain the thiophene structure shown below; then adding the solution containing the polyfluorene polymer in step T1, reacting at room temperature for a period of time, and obtaining the polyfluorene-polythiophene block copolymer after post-treatment; 10. The method for preparing polyfluorene-polythiophene block copolymer nanowires according to claim 9, characterized in that: The post-treatment operation in step T2 is to add ether to the reaction solution to terminate the reaction, wash the obtained product with ether for 4-5 times, and vacuum dry it until the mass remains unchanged.

Citation Information

Patent Citations

  • Diaryl fluorine pi accumulated small molecule organic nanostructure and transistorized memory thereof

    CN103663365A

  • Block copolymers that disperse nanofilaments in water

    CN104428367A

  • Full-conjugated block polyelectrolyte and preparation method thereof

    CN104804176A

  • Block copolymer composition, self-assembled structure of block copolymer

    KR102219498B1

  • Process for preparation of conducting polymers

    US20100234478A1