Triazine ultraviolet absorbent and preparation method thereof
By introducing polyethylene glycol chains and hydroxyl groups into triazine-type ultraviolet absorbers, the incompatibility and performance inconsistency of light stabilizers in polymer materials are solved, the water solubility and color uniformity of the material are improved, and the water solubility and color uniformity of the material are extended. The service life of the material.
Patent Information
- Application Number
- CN202411290958.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-15
AI Technical Summary
Existing light stabilizers have problems such as incompatibility, uneven fusion, uneven color and inconsistent performance in polymer polymer materials, which leads to aging of the material and affects its use value.
Polyethylene glycol chains are introduced into the chain structure of triazine-type ultraviolet absorbers and hydroxyl groups are introduced at the end of the chain to improve compatibility and mixing properties with the polymer structure.
It improves water solubility, solves the incompatibility and performance inconsistency between polymers and additives, and improves the color uniformity and crack resistance of the material.
Smart Images

Figure CN118955888A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of functional additives for polymer materials, and in particular to a triazine ultraviolet absorber and a preparation method thereof. Background Art
[0002] Polymer materials usually exist in the form of polymers, such as plastics, coatings, dyes, artificial fibers, and artificial rubber. These polymer materials are exposed to sunlight for a long time and are easily aging due to ultraviolet rays, such as common discoloration, cracking and peeling of coatings, fading and fading, etc. In more serious cases, the material texture becomes brittle, the toughness decreases, and the elongation performance weakens. Once the material product ages, it will soon lose its use value.
[0003] Light stabilizers are additives that inhibit or slow down the degradation of polymer materials caused by photooxidation. With polymer materials being widely used in the fields of communications, energy, chemicals, and communication equipment, light stabilizers have also developed into an important category of polymer material additives. Triazine UV absorbers are a relatively new type of light stabilizer. This type of compound has a larger molecular structure and excellent UV absorption performance. It has strong absorption of UVA and UVB ultraviolet rays. In addition, this type of absorber also has certain antioxidant properties. Triazine UV absorbers have good thermal stability, high-efficiency UV absorption performance, and broad-spectrum UV absorption characteristics. Therefore, this type of absorber has received widespread attention and recognition in the market.
[0004] Currently, most of the light stabilizers on the market are added to polymers in the form of foreign substances, which may cause incompatibility between polymers and additives, uneven fusion, a foreign body feeling in the polymer, uneven color, cracking, inconsistent performance and other problems.
[0005] Water-based light stabilizers use water as solvent, which saves a lot of resources and eliminates the risk of fire during construction; it reduces air pollution and only uses a small amount of low-toxic alcohol ether organic solvents, which improves the working environment. Therefore, the market demand for water-based light stabilizers has grown more and more significantly in recent years. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a triazine ultraviolet absorber and a preparation method thereof. The present invention introduces a polyethylene glycol chain into the chain structure of the triazine ultraviolet absorber for the first time, which increases the water solubility of the structure and introduces a hydroxyl group at the end of the chain, which can be bonded to the main chain of the polymer structure, thereby improving the problems of incompatibility between the polymer and the auxiliary agent, uneven fusion, foreign body sensation in the polymer, uneven color, cracking, inconsistent performance, etc.
[0007] The technical solution of the present invention is as follows:
[0008] The first aspect of the present invention protects a triazine ultraviolet absorber, the structure of the triazine ultraviolet absorber is shown in general formula (1) or general formula (2);
[0009]
[0010] in:
[0011] R1 and R2 are independently hydrogen, substituted or unsubstituted C1-C 10 The alkyl group;
[0012] n1≥0; n2≥0;
[0013] The substituents for the substituent groups are selected from deuterium atoms, tritium atoms, halogen atoms, C1-C 10 One or more of the alkyl groups.
[0014] Further, R1 and R2 are independently represented by one of hydrogen, methyl, ethyl, propyl, butyl, deuterated methyl, tritiated methyl, trifluoromethyl, trichloromethyl, deuterated ethyl, tritiated ethyl, isopropyl, deuterated isopropyl, tritiated isopropyl, tert-butyl, deuterated tert-butyl, tritiated tert-butyl, cyclopentyl, deuterated cyclopentyl, tritiated cyclopentyl, methyl-substituted cyclopentyl, and cyclohexyl; n1≥10; n2≥1.
[0015] The second aspect of the present invention protects a method for preparing the triazine ultraviolet absorber described in the first aspect, comprising the following steps:
[0016] S1: Compound (1), compound (2) and a base are added to solvent I, and after reaction, post-treatment is performed to obtain an intermediate compound (3).
[0017] S2: adding the intermediate compound (3), diol and catalyst into solvent II, reacting and post-treating to obtain a triazine ultraviolet absorber, namely, a compound represented by general formula (1) or general formula (2).
[0018] Wherein, the structural formula of the compound (1) is shown as formula (m1) or formula (m2), the structural formula of the compound (2) is shown as formula (m3); the structural formula of the intermediate compound (3) is shown as formula (m4) or formula (m5).
[0019]
[0020] In the general formula (m3) to the general formula (m5), R1 and R3 are independently hydrogen, substituted or unsubstituted C1-C 10 The substituents for the substituent group are selected from deuterium atoms, tritium atoms, halogen atoms, C1~C 10one or more of the alkyl groups; X is a halogen; and, when the triazine ultraviolet absorber is a compound represented by the general formula (1), the structural formula of the compound (1) is (m1), and the structural formula of the intermediate compound (3) is the general formula (m4); when the triazine ultraviolet absorber is a compound represented by the general formula (2), the structural formula of the compound (1) is (m2), and the structural formula of the intermediate compound (3) is the general formula (m5).
[0021] Further, R1 and R3 are independently represented by one of hydrogen, methyl, ethyl, propyl, butyl, deuterated methyl, tritiated methyl, trifluoromethyl, trichloromethyl, deuterated ethyl, tritiated ethyl, isopropyl, deuterated isopropyl, tritiated isopropyl, tert-butyl, deuterated tert-butyl, tritiated tert-butyl, cyclopentyl, deuterated cyclopentyl, tritiated cyclopentyl, methyl-substituted cyclopentyl, and cyclohexyl; and X is selected from one of Cl, Br, and I.
[0022] Furthermore, in step S1, the solvent I is selected from one or more of toluene, xylene, chlorobenzene, nitrobenzene, dichloromethane, acetonitrile, tetrahydrofuran, 1,4-dioxane, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; and the mass volume ratio of the compound (1) to the solvent I is 100:500-1500 g / mL.
[0023] Furthermore, in step S1, the base is selected from at least one of potassium carbonate, sodium carbonate, sodium bicarbonate, triethylamine, diethylisopropylamine, and pyridine; the molar ratio of compound (1), compound (2) and base is 1:0.05-5:1-5; preferably 1:1-5:1-5, more preferably 1:1.1:1.1.
[0024] Furthermore, in step S1, the reaction temperature is 0-120°C and the reaction time is 0.5-24h.
[0025] Furthermore, in step S2, the catalyst is selected from at least one of calcium acetate, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and dodecylbenzenesulfonic acid; the diol includes at least one of diethylene glycol and polyethylene glycol; and the solvent II includes at least one of toluene or xylene, tetrahydrofuran, 1,4-dioxane, dichloromethane, and acetonitrile.
[0026] Furthermore, in step S2, the molar ratio of the intermediate compound (3), polyethylene glycol and catalyst is 1:1-5:0.05-1, preferably 1:2:0.2; the mass volume ratio of the intermediate compound (3) to solvent II is 1:10-20 g / mL.
[0027] Furthermore, in step S2, the reaction temperature is 80-110° C. and the reaction time is 0.5-48 h.
[0028] The beneficial technical effects of the present invention are:
[0029] The invention introduces a polyethylene glycol chain into the chain structure of a triazine ultraviolet absorber, which increases the water solubility of the structure and introduces a hydroxyl group at the end of the chain to bond to the main chain of the polymer structure, thereby improving problems such as incompatibility between the polymer and the auxiliary agent, uneven fusion, a foreign body feeling in the polymer, uneven color, cracking, inconsistent performance, and the like.
[0030] The preparation method of the novel triazine ultraviolet absorber of the present invention is simple to operate and has a high yield of the target product. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the UV absorption diagram of the compounds prepared in Examples 1-4 of the present invention.
[0032] Figure 2 This is the UV absorption diagram of the compound prepared in Example 5 of the present invention.
[0033] Figure 3 It is the hydrogen spectrum of compound a in Example 1 of the present invention.
[0034] Figure 4 It is the hydrogen spectrum of compound b in Example 2 of the present invention.
[0035] Figure 5 It is the hydrogen spectrum of compound c in Example 3 of the present invention.
[0036] Figure 6 It is the hydrogen spectrum of compound d in Example 4 of the present invention.
[0037] Figure 7 This is the hydrogen spectrum of compound e in Example 5 of the present invention.
[0038] Figure 8 This is the MS chart of compound a in Example 1 of the present invention. DETAILED DESCRIPTION
[0039] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0040] The first aspect of the present invention provides a triazine ultraviolet absorber, the structure of the triazine ultraviolet absorber is shown in general formula (1) or general formula (2);
[0041]
[0042] in:
[0043] R1 and R2 are independently hydrogen, substituted or unsubstituted C1-C 10alkyl; n1≥0; n2≥0; the substituents for the substituent group are selected from deuterium atoms, tritium atoms, halogen atoms, C1~C 10 One or more of the alkyl groups.
[0044] In some embodiments, R1 and R2 are independently represented by one of hydrogen, methyl, ethyl, propyl, butyl, deuterated methyl, tritiated methyl, trifluoromethyl, trichloromethyl, deuterated ethyl, tritiated ethyl, isopropyl, deuterated isopropyl, tritiated isopropyl, tert-butyl, deuterated tert-butyl, tritiated tert-butyl, cyclopentyl, deuterated cyclopentyl, tritiated cyclopentyl, methyl-substituted cyclopentyl, and cyclohexyl; preferably, R1 is represented by at least one of hydrogen, methyl, and ethyl; R2 is represented by at least one of hydrogen, methyl, and ethyl; R1 and R2 are the same or different.
[0045] In some embodiments, n1≥10; n2≥1. It is understood that in the present invention, when n1≥10, the obtained product has good hydrophobicity. When n2≥0, the product has hydrophilicity.
[0046] The second aspect of the present invention protects a method for preparing the triazine ultraviolet absorber described in the first aspect, wherein when the triazine ultraviolet absorber is a compound described in general formula (1), the preparation method comprises the following steps:
[0047] S1: Compound (1), compound (2) and a base are added to solvent I, and after reaction, post-treatment is performed to obtain an intermediate compound (3).
[0048] S2: adding the intermediate compound (3), diol and catalyst into solvent II, reacting and post-treating to obtain a triazine ultraviolet absorber, namely, the compound represented by general formula (1).
[0049] The structural formula of the compound (1) is shown in formula (m1), the structural formula of the compound (2) is shown in formula (m3); and the structural formula of the intermediate compound (3) is shown in formula (m4).
[0050]
[0051] In the general formula (m3) to the general formula (m4), R1 and R3 are independently hydrogen, substituted or unsubstituted C1-C 10 The substituents for the substituent group are selected from deuterium atoms, tritium atoms, halogen atoms, C1~C 10 One or more of the alkyl groups; X is a halogen.
[0052] In some embodiments, R1 and R3 are independently represented by one of hydrogen, methyl, ethyl, propyl, butyl, deuterated methyl, tritiated methyl, trifluoromethyl, trichloromethyl, deuterated ethyl, tritiated ethyl, isopropyl, deuterated isopropyl, tritiated isopropyl, tert-butyl, deuterated tert-butyl, tritiated tert-butyl, cyclopentyl, deuterated cyclopentyl, tritiated cyclopentyl, methyl-substituted cyclopentyl, and cyclohexyl; and X is selected from one of Cl, Br, and I.
[0053] In some embodiments, in step S1, the solvent I is selected from one or more of toluene, xylene, chlorobenzene, nitrobenzene, dichloromethane, acetonitrile, tetrahydrofuran, 1,4-dioxane, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; and the mass volume ratio of the compound (1) to the solvent I is 100:500-1500 g / mL.
[0054] In some embodiments, in step S1, the base is selected from at least one of potassium carbonate or sodium carbonate, sodium bicarbonate, triethylamine diethylisopropylamine, and pyridine; the molar ratio of compound (1), compound (2) and base is 1:1-5:0.05-5; including but not limited to 1:1:0.05, 1:1:1, 1:5:5, 1:5:1, 1:2:2, 1:2:5, 1:3:4, preferably 1:1-5:1-5, more preferably 1:1.1:1.1.
[0055] In some embodiments, in step S1, the reaction temperature is 0-120°C, and the time is 0.5-24h, and the temperature includes but is not limited to 5°C, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C; the time includes but is not limited to 0.5h, 1h, 10h, 15h, 20h, 22h, 24h.
[0056] In some embodiments, in step S1, the post-treatment includes removing most of the toluene under reduced pressure after the reaction is complete by TLC detection, adding water, stirring, filtering, collecting solids, and then slurrying the solids with n-heptane and drying.
[0057] In some trial methods, in step S2, the catalyst is selected from at least one of calcium acetate, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and dodecylbenzenesulfonic acid; the diol includes at least one of diethylene glycol and polyethylene glycol. Preferably, the polyethylene glycol includes at least one of polyethylene glycol 400, polyethylene glycol 600, and polyethylene glycol 1000. The polyethylene glycol 400, polyethylene glycol 600, and polyethylene glycol 1000 described in the present invention are all from Shanghai Bid Pharmaceutical Technology Co., Ltd. The solvent II includes at least one of toluene or xylene, tetrahydrofuran, 1,4-dioxane, dichloromethane, and acetonitrile.
[0058] In some embodiments, in step S2, the molar ratio of the intermediate compound (3), polyethylene glycol and catalyst is 1:1-5:0.05-1; including but not limited to 1:1:0.1, 1:5:1, 1:5:0.1, 1:2:0.1, 1:2:1, 1:3:1, preferably 1:1-5:0.1-1, more preferably 1:2:0.2. The mass volume ratio of the intermediate compound (3) to the solvent II is g / mL 1:10-20, including but not limited to 1:10, 1:12, 1:16, 1:18, 1:20.
[0059] In some embodiments, in step S2, the reaction temperature is 80-110°C, and the reaction time is 0.5-48h; the time includes but is not limited to 0.5h, 1h, 10h, 15h, 20h, 25h, 30h, 35h, 40h, 45h, 48h.
[0060] In some embodiments, in step S2, the post-treatment includes removing most of the toluene under reduced pressure after the reaction is complete by TLC detection, adding water, stirring, filtering, collecting solids, and then slurrying the solids with n-heptane and drying.
[0061] In some embodiments, when the triazine ultraviolet absorber is a compound of formula (2), the preparation method thereof comprises the following steps:
[0062] S1: Compound (1), compound (2) and a base are added to solvent I, and after reaction, post-treatment is performed to obtain an intermediate compound (3).
[0063] S2: adding the intermediate compound (3), polyethylene glycol and a catalyst into solvent II, reacting and post-treating to obtain a triazine ultraviolet absorber, namely, a compound represented by general formula (1) or general formula (2).
[0064] The structural formula of the compound (1) is shown in formula (m2), the structural formula of the compound (2) is shown in formula (m3); and the structural formula of the intermediate compound (3) is shown in general formula (m5).
[0065]
[0066] In the general formula (m3) and the general formula (m5), R1 and R3 are independently hydrogen, substituted or unsubstituted C1-C 10 The substituents for the substituent group are selected from deuterium atoms, tritium atoms, halogen atoms, C1~C 10 One or more of the alkyl groups; X is a halogen.
[0067] In some embodiments, R1 and R3 are independently represented by one of hydrogen, methyl, ethyl, propyl, butyl, deuterated methyl, tritiated methyl, trifluoromethyl, trichloromethyl, deuterated ethyl, tritiated ethyl, isopropyl, deuterated isopropyl, tritiated isopropyl, tert-butyl, deuterated tert-butyl, tritiated tert-butyl, cyclopentyl, deuterated cyclopentyl, tritiated cyclopentyl, methyl-substituted cyclopentyl, and cyclohexyl; and X is selected from one of Cl, Br, and I.
[0068] In some embodiments, in step S1, the solvent I is selected from one or more of toluene, xylene, chlorobenzene, nitrobenzene, dichloromethane, acetonitrile, tetrahydrofuran, 1,4-dioxane, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; and the mass volume ratio of the compound (1) to the solvent I is 100:500-1500 g / mL.
[0069] In some embodiments, in step S1, the base is selected from at least one of potassium carbonate or sodium carbonate, sodium bicarbonate, triethylamine diethylisopropylamine, and pyridine; the molar ratio of compound (1), compound (2) and base is 1:1-5:0.05-5; including but not limited to 1:1:1, 1:5:5, 1:5:1, 1:2:2, 1:2:5, 1:3:4, preferably 1:1-5:1-5, more preferably 1:1.1:1.1.
[0070] In some embodiments, in step S1, the reaction temperature is 0-120°C, and the time is 0.5-24h, and the temperature includes but is not limited to 5°C, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C; the time includes but is not limited to 0.5h, 1h, 10h, 15h, 20h, 22h, 24h.
[0071] In some embodiments, in step S2, the catalyst is selected from at least one of calcium acetate or methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and dodecylbenzenesulfonic acid. The diol includes at least one of diethylene glycol and polyethylene glycol. Preferably, the polyethylene glycol includes at least one of polyethylene glycol 400, polyethylene glycol 600, and polyethylene glycol 1000. The polyethylene glycol 400, polyethylene glycol 600, and polyethylene glycol 1000 described in the present invention are all from Shanghai Bid Pharmaceutical Technology Co., Ltd. The solvent II includes at least one of toluene or xylene, tetrahydrofuran, 1,4-dioxane, dichloromethane, and acetonitrile.
[0072] In some embodiments, in step S2, the molar ratio of the intermediate compound (3), polyethylene glycol and catalyst is 1:1-5:0.05-1; including but not limited to 1:1:0.1, 1:5:1, 1:5:0.1, 1:2:0.1, 1:2:1, 1:3:1, preferably 1:1-5:0.1-1, more preferably 1:2:0.2. The mass volume ratio of the intermediate compound (3) to the solvent II is g / mL 1:10-20, including but not limited to 1:10, 1:12, 1:16, 1:18, 1:20.
[0073] In some embodiments, in step S2, the reaction temperature is 80-110°C, and the reaction time is 0.5-48h; the time includes but is not limited to 0.5h, 1h, 10h, 15h, 20h, 25h, 30h, 35h, 40h, 45h, 48h.
[0074] It is understood that the triazine compounds of the present invention can be used as ultraviolet absorbers alone or as components of ultraviolet absorbers. It is understood that the triazine compounds prepared by the present invention increase the water solubility of the triazine ultraviolet absorbers by introducing polyethylene glycol chains into the chain structure of the triazine ultraviolet absorbers to obtain compounds containing hydroxyl groups at the chain ends. At the same time, the terminal hydroxyl groups can react with the polymer. The molecular chains of the substances react to form a bond. The compatibility of polymer and additives is improved, as well as the color uniformity and crack resistance of the polymer and additive mixture.
[0075] The present invention will be further described below by way of examples and the like.
[0076] Example 1
[0077] A novel triazine ultraviolet absorber a, whose structural formula is as follows:
[0078]
[0079] The synthetic route of the novel triazine ultraviolet absorber a is as follows:
[0080]
[0081] The synthesis method of the novel triazine ultraviolet absorber a specifically comprises the following steps:
[0082] (1) Preparation of compound a2
[0083] 100.00 g of compound a1 (0.252 mol), 32.80 g of methyl chloroformate (0.302 mol) and 19.35 g of sodium bicarbonate were added to 1000 mL of toluene solution, heated to 60°C and refluxed for reaction for 5 h. After TLC detection showed that the reaction was complete, most of the toluene was removed under reduced pressure, water was added, stirred, filtered, and the solid was collected. The solid was then slurried with n-heptane and dried to obtain 106 g of a light yellow solid of compound a2 with a yield of 90%.
[0084] (2) Preparation of compound a
[0085] 100.00 g of compound a2 (0.213 mol), 67.73 g of diethylene glycol (0.639 mol) and 2.00 g of methanesulfonic acid were added to 1000 ml of toluene solution, heated to 90°C and refluxed for reaction for 16 h. After TLC detection showed that the reaction was complete, most of the toluene was removed under reduced pressure, water was added, stirred, filtered, and the solid was collected. The solid was then slurried with n-heptane and dried to obtain 108 g of compound a as a light yellow solid with a yield of 93%.
[0086] pass 1 The obtained light yellow solid product a was characterized by H NMR and MS. Figure 3 and Figure 8 As shown, the obtained data are as follows:
[0087] 1 H NMR(400MHz,Chloroform-d)δ13.47(s,1H),8.54(d,J=8.9Hz,1H),8.07(s,2H),7.18(d,J=6.7Hz,4H),6.63(dd,J=8.9,2.6Hz,1H) ,6.49(d,J=2.5Hz,1H),4.74(s,2H),4.51–4.33(m,2H),3.75(dd,J=5.5,3.6Hz,4H),3.67–3.52(m,2H),2.74(s,6H),2.41(s,6H).
[0088] ESI-MS(positive mode,m / z)found(calcd)for[M] + :543.7(544.2).
[0089] By the above 1The results of H NMR and MS analysis confirmed that the light yellow solid product prepared in this example was a novel triazine ultraviolet absorber a.
[0090] Example 2
[0091] Triazine UV absorber b, its structural formula is as follows:
[0092]
[0093] The synthetic route of triazine UV absorber b is as follows:
[0094]
[0095] The preparation method of triazine ultraviolet absorber b is as follows:
[0096] (1) Compound a2 was prepared according to the method described in Example 1;
[0097] (2) 10.00 g of compound a2 (0.021 mol), 25.6 g of polyethylene glycol 400 and 0.20 g of methanesulfonic acid were added to 200 mL of toluene solution, heated to 90° C. and refluxed for 16 h. After the reaction was completed as detected by TLC, most of the toluene was removed under reduced pressure and column chromatography (DCM / MeOH) was performed to obtain 14.6 g of compound b as a light yellow oily solid with a yield of 80%.
[0098] pass 1 The obtained light yellow solid product was characterized by H NMR. Figure 4 As shown, the obtained data is as follows:
[0099] 1 H NMR(400MHz,Chloroform-d)δ13.41(s,1H),8.53(d,J=9.0Hz,1H),8.06(m,2H),7.18(d,J=6.5Hz,4H),6.62(dd,J=9.0,2.6Hz,1H),6.48(d,J=2.6Hz ,1H),4.74(d,J=4.8Hz,2H),4.45–4.36(m,2H),4.37–4.27(m,2H),3.73(d dd,J=8.7,5.4,2.9Hz,7H),3.65–3.58(m,30H),2.74(s,6H),2.41(s,6H).
[0100] By the above 1 The results of H NMR analysis confirmed that the light yellow oily solid product prepared in this example was the novel triazine ultraviolet absorber b.
[0101] Example 3
[0102] Triazine UV absorber c has the following structural formula:
[0103]
[0104] The synthetic route of triazine UV absorber c is as follows:
[0105]
[0106] The preparation method of triazine ultraviolet absorber c comprises the following steps:
[0107] (1) Compound a2 was prepared according to the method described in Example 1;
[0108] (2) 10.00 g of compound a2 (0.021 mol), 37.80 g of polyethylene glycol 600 and 0.20 g of methanesulfonic acid were added to 200 ml of toluene solution, heated to 90°C and refluxed for 16 h. After the reaction was completed as detected by TLC, most of the toluene was removed under reduced pressure and column chromatography (DCM / MeOH) was performed to obtain 16.6 g of compound c as a light yellow oily solid with a yield of 75%.
[0109] pass 1 The obtained light yellow solid product c was characterized by H NMR. Figure 5 As shown, the obtained data are as follows:
[0110] 1 H NMR(400MHz,Chloroform-d)δ13.40(s,1H),8.52(d,J=9.0Hz,1H),8.07(d,J=8.5Hz,2H),7.17(d,J=6.4Hz,4H ),6.61(dd,J=8.9,2.6Hz,1H),6.47(d,J=2.6Hz,1H),4.72(d,J=3.8Hz,2H),4.38(dd,J=5.6,3.8Hz,2H),4.35–
[0111] 4.27(m,2H),3.71(dt,J=7.1,2.7Hz,8H),3.63(d,J=2.4Hz,44H),2.73(s,6H),2.40(s,6H).
[0112] By the above 1 The results of H NMR analysis confirmed that the light yellow oily solid product prepared in this example was the novel triazine ultraviolet absorber c.
[0113] Example 4
[0114] Triazine UV absorber d, its structural formula is as follows:
[0115]
[0116] The synthetic route of triazine UV absorber d is as follows:
[0117]
[0118] The preparation method of triazine ultraviolet absorber d is as follows:
[0119] (1) Compound a2 was prepared according to the method described in Example 1.
[0120] (2) 10.00 g of compound a2 (0.021 mol), 63.00 g of polyethylene glycol 1000 and 0.20 g of methanesulfonic acid were added to 200 mL of toluene solution, heated to 90° C. and refluxed for 16 h. After the reaction was completed as detected by TLC, most of the toluene was removed under reduced pressure and column chromatography (DCM / MeOH) was performed to obtain 18.3 g of compound d as a light yellow oily solid with a yield of 60%.
[0121] pass 1 The obtained light yellow solid product was characterized by H NMR. Figure 6 As shown, the obtained data are as follows:
[0122] 1 H NMR(400MHz,Chloroform-d)δ13.40(s,1H),8.53(d,J=9.0Hz,1H),8.06(s,2H),7.18(d,J=6.5Hz,3H),6.61(dd,J=9.0,2.5Hz,1 H),6.48(d,J=2.6Hz,1H),4.72(s,2H),4.45–4.32(m,2H),3.78–3.69(m,8H),3.63(d,J=3.7Hz,80H),2.74(s,6H),2.41(s,6H).
[0123] By the above 1 The results of H NMR analysis confirmed that the light yellow oily solid product prepared in this example was the novel triazine ultraviolet absorber d.
[0124] Example 5
[0125] Triazine UV absorber e, its structural formula is as follows:
[0126]
[0127] The synthesis route of the novel triazine ultraviolet absorber e is as follows:
[0128]
[0129] (1) 100.00 g of compound e1 (0.252 mol), 32.80 g of methyl chloroformate (0.302 mol) and 19.35 g of sodium bicarbonate were added to 1000 mL of toluene solution, heated to 60° C. and refluxed for reaction for 5 h. After TLC detection showed that the reaction was complete, most of the toluene was removed under reduced pressure, water was added, stirred, filtered, and the solid was collected. The solid was then slurried with n-heptane and dried to obtain 106 g of a light yellow solid of compound e2 with a yield of 90%.
[0130] (2) 10.00 g of compound e2 (0.015 mol), 4.80 g of diethylene glycol and 0.15 g of methanesulfonic acid were added to 100 mL of toluene solution, heated to 90° C. and refluxed for 16 h. After the reaction was completed as detected by TLC, most of the toluene was removed under reduced pressure and column chromatography (DCM / MeOH) was performed to obtain 6.64 g of compound e as a light yellow oily solid, with a yield of 50%.
[0131] pass 1 The obtained light yellow solid product e was characterized by H NMR. Figure 7 As shown, the obtained data are as follows:
[0132] 1 H NMR (400MHz, Chloroform-d) δ13.49(s,3H),7.90(d,J=9.0Hz,3H),6.49(d,J=9.1Hz,3H),4.72(s,6H),4.22(m,6H),3.79–3.68(m,8H).
[0133] By the above 1 The results of H NMR analysis confirmed that the light yellow oily solid product prepared in this example was a novel triazine ultraviolet absorber e.
[0134] Performance Test:
[0135] (1) UV absorption performance test
[0136] Compound a, compound b, compound c, compound d and compound e prepared in Examples 1-5 were prepared into 0.005% chloroform solution, and the transmission spectra of each compound were tested to evaluate its absorption performance. The results are as follows: Figure 1-2 As shown in the figure, it can be seen that compound a, compound b, compound c and compound d have good ultraviolet absorption function in the range of 280nm to 350nm, and compound e has good ultraviolet absorption function in the range of 320nm to 380nm.
[0137] (2) Hydrophilicity test
[0138] Compound a, compound b, compound c, compound d and compound e prepared in the examples were mixed with water to make a 5% solution (the ratio of the ultraviolet absorber is generally less than 5%), and the hydrophilicity of each compound was tested. The results are as follows:
[0139] Table 1: Hydrophilicity test of the compounds prepared in the examples
[0140] name Compound a Compound b Compound c Compound d Compound e Solubility Insoluble Gel-like Dissolve Dissolve Dissolve
[0141] It can be seen from the above table that compound c, compound d and compound e have good hydrophilicity and can be used as water-based ultraviolet absorbers.
[0142] The above is only a preferred embodiment of the present invention, and the present invention is not limited to the above embodiments. It is understood that other improvements and changes directly derived or associated by those skilled in the art without departing from the spirit and concept of the present invention should be considered to be included in the protection scope of the present invention.
Claims
1. A triazine ultraviolet absorber, characterized in that: The structure of the triazine ultraviolet absorber is shown in general formula (1) or general formula (2); in: R1 and R2 are independently hydrogen, substituted or unsubstituted C1-C 10 The alkyl group; n1≥0; n2≥0; The substituents for the substituent groups are selected from deuterium atoms, tritium atoms, halogen atoms, C1-C 10 One or more of the alkyl groups.
2. The triazine ultraviolet absorber according to claim 1, characterized in that: R1 and R2 are independently selected from the group consisting of hydrogen, methyl, ethyl, propyl, butyl, deuterated methyl, tritiated methyl, trifluoromethyl, trichloromethyl, deuterated ethyl, tritiated ethyl, isopropyl, deuterated isopropyl, tritiated isopropyl, tert-butyl, deuterated tert-butyl, tritiated tert-butyl, cyclopentyl, deuterated cyclopentyl, tritiated cyclopentyl, methyl-substituted cyclopentyl, and cyclohexyl; The n1≥10; the n2≥1.
3. A method for preparing the triazine ultraviolet absorber according to any one of claims 1 to 2, characterized in that: The steps include: S1: adding compound (1), compound (2) and a base into solvent I, reacting, and then post-treating to obtain an intermediate compound (3); S2: adding the intermediate compound (3), diol and catalyst into solvent II for reaction, and obtaining a triazine ultraviolet absorber through post-treatment, i.e., a compound represented by general formula (1) or general formula (2); Wherein, the structural formula of the compound (1) is shown in formula (m1) or formula (m2), the structural formula of the compound (2) is shown in formula (m3); the structural formula of the intermediate compound (3) is shown in formula (m4) or formula (m5); and, When the triazine ultraviolet absorber is a compound represented by the general formula (1), the structural formula of the compound (1) is (m1), the structural formula of the intermediate compound (3) is the general formula (m4), When the triazine ultraviolet absorber is a compound represented by the general formula (2), the structural formula of the compound (1) is (m2), and the structural formula of the intermediate compound (3) is the general formula (m5); In general formula (m3) to general formula (m5): R1 and R3 are independently hydrogen, substituted or unsubstituted C1-C 10 The alkyl group; The substituents for the substituent groups are selected from deuterium atoms, tritium atoms, halogen atoms, C1-C 10 One or more of the alkyl groups of X is halogen.
4. The preparation method according to claim 3, characterized in that: R1 and R3 are independently selected from the group consisting of hydrogen, methyl, ethyl, propyl, butyl, deuterated methyl, tritiated methyl, trifluoromethyl, trichloromethyl, deuterated ethyl, tritiated ethyl, isopropyl, deuterated isopropyl, tritiated isopropyl, tert-butyl, deuterated tert-butyl, tritiated tert-butyl, cyclopentyl, deuterated cyclopentyl, tritiated cyclopentyl, methyl-substituted cyclopentyl, and cyclohexyl; X is selected from the group consisting of Cl, Br, and I.
5. The preparation method according to claim 3, characterized in that: In step S1, the solvent I is selected from one or more of toluene, xylene, chlorobenzene, nitrobenzene, dichloromethane, acetonitrile, tetrahydrofuran, 1,4-dioxane, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; The mass volume ratio of the compound (1) to the solvent I is 100:500-1500 g / mL.
6. The preparation method according to claim 3, characterized in that: In step S1, the base is selected from at least one of potassium carbonate, sodium carbonate, sodium bicarbonate, triethylamine, diethylisopropylamine, and pyridine; The molar ratio of the compound (1), the compound (2) and the base is 1:1-5:0.05-5; preferably 1:1.1:1.
1.
7. The preparation method according to claim 3, characterized in that: In step S1, the reaction temperature is 0-120°C and the reaction time is 0.5-24h.
8. The preparation method according to claim 3, characterized in that: In step S2, the catalyst is selected from at least one of calcium acetate, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and dodecylbenzenesulfonic acid; the diol includes at least one of diethylene glycol and polyethylene glycol; the solvent II includes at least one of toluene or xylene, tetrahydrofuran, 1,4-dioxane, dichloromethane, and acetonitrile.
9. The preparation method according to claim 3, characterized in that: In step S2, the molar ratio of the intermediate compound (3), polyethylene glycol and catalyst is 1:1-5:0.05-1, preferably 1:2:0.2; the mass volume ratio of the intermediate compound (3) to solvent II is 1:10-20 g / mL.
10. The preparation method according to claim 3, characterized in that: In step S2, the reaction temperature is 80-110° C. and the reaction time is 0.5-48 h.
Citation Information
Cited By
Anti-aging polyvinyl chloride sheet and preparation method thereof
CN119735902A