Micro-electric bionic dynamic expelling antifouling surface and preparation method thereof

Through microelectrobionics dynamically drive away the anti-fouling surface, and using electroosmotic flow and microfluid flow mechanisms to simulate the anti-fouling structure of the skin of the cetaceans, it solves the shortcomings of the existing marine anti-fouling technology in broad spectrum and long-term effectiveness, and achieves the Low energy consumption and efficient anti-fouling effect, suitable for a variety of marine applications.

CN118955977APending Publication Date: 2024-11-15JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410871261.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

It is difficult for existing marine anti-fouling technology to achieve unity in broad spectrum and long-term effectiveness. Traditional toxic anti-fouling agents have negative impacts on the environment. Environmentally friendly anti-fouling surfaces have limited effects in actual applications, especially in low hydrodynamic conditions.

Method used

Microelectrobionics dynamically drive away the anti-fouling surface, and is composed of ion exchange membrane, electrode material and low-surface energy anti-fouling layer. The anti-fouling structure of the skin of cetaceans is simulated by electroosmotic flow and microfluidic flow mechanism to achieve dynamic removal and Anti-fouling effect.

Benefits of technology

This technology can achieve efficient anti-fouling at low voltage, destroy the microbial growth environment, prevent microbial adhesion, reduce biofilm formation, and has low energy consumption. It is suitable for ships, seawater pipelines and high-performance marine equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955977A_ABST
    Figure CN118955977A_ABST
Patent Text Reader

Abstract

The invention provides a micro-electric bionic dynamic expelling antifouling surface and a preparation method thereof. The antifouling surface takes a dynamic epidermis structure of whale-dolphin skin as a bionic prototype, can simulate reversible macroscopic mechanical deformation and micro-fluid disturbance of the whale-dolphin skin under the action of external electrical stimulation, and effectively prevents microorganisms from being adhered to the surface of the material. The antifouling surface is prepared from an ion exchange membrane, an electrode and an antifouling surface layer material with low surface energy. Since the antifouling surface is constructed based on the ion migration effect, the surface can be at ultra-low voltage (lt; 3V), and excellent deformation performance can be realized. The anti-fouling surface belongs to pure physical anti-biological fouling, so that the harm of biochemical reagents to the environment is avoided. The antifouling mechanism driven by ion migration allows the antifouling effect to be dynamically controlled, and the antifouling performance in different environments is optimized by adjusting voltage and current. The technology is particularly suitable for high-tech equipment and environment sensitive areas requiring self-adaptive antifouling capability, such as ocean exploration and ocean motion equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of marine antifouling functional surfaces, and in particular relates to a micro-electric bionic dynamic antifouling surface. Background Art

[0002] Marine biofouling refers to the attachment and growth of fouling organisms (such as bacteria, algae, barnacles, etc.) on underwater surfaces. The problem of marine biofouling has been hindering the pace of human exploration of the ocean since ancient times. Today, with the prosperity of global shipping trade, the economic losses and environmental problems caused by the large-scale accumulation of marine organisms on the surfaces of marine equipment such as ships, docks, drilling platforms, and cross-sea bridges are becoming more and more serious. The main consequences are: ① Increase the weight and surface roughness of underwater equipment, significantly increase navigation resistance and fuel consumption, and bring about a substantial increase in operating costs. Studies have shown that even if there is mild biofouling in the form of mucus film on the surface of the ship, it will increase the shaft power required to overcome additional resistance and maintain operating speed by 11%. In contrast, if biofouling produces heavy calcium deposits, the power loss of the ship will be as high as 86%. ② Excessive fuel consumption increases the emission of greenhouse gases and harmful gases such as carbon dioxide, sulfur oxides and nitrogen oxides, which ultimately affects the climate environment and endangers human health. ③ Change the local microenvironment of the underwater surface, accelerate the surface corrosion rate, and affect the safety of underwater equipment. ④ Cause biological invasion. Fouling organisms travel around the world with ships. When they reach new waters without natural enemies, they are likely to cause biological invasion and endanger the local ecological environment.

[0003] The formation process of biofouling can usually be divided into four stages: ① Formation of conditional film: In the first few seconds after the material surface is immersed in seawater, inorganic and organic macromolecules (such as proteins) will be adsorbed through physical action. This stage will form the basic environment for the survival of microorganisms, which is the first step of biological adhesion. The duration of this stage depends on the physicochemical properties of the solid material surface, such as surface roughness, chemical composition, etc. ② Reversible adhesion and colonization stage of microorganisms: In the next few hours, bacteria, algae and other microorganisms migrate to the surface and secrete extracellular polymers (EPS) to promote adhesion and form biofilms. Bacteria and algae can detach from the surface under the action of external forces, so this process is reversible. ③ Irreversible adhesion and aggregation stage: In the next few days, multicellular organisms (such as large algae and protozoan spores) reach the surface, and then begin to grow and reproduce in large quantities, and secrete harmful substances, accelerating the corrosion rate of underwater surfaces. ④ Biofilm maturation and recolonization stage: In the next few weeks, the biofilm has been formed and stabilized, some animal larvae begin to gather (such as barnacles and mussels), and their impact on the facilities gradually reaches a peak. The above biofouling formation process is generally accepted by researchers, but it is also affected by the sea area, season, and type of fouling organisms. Some stages will overlap or occur in parallel. In general, interfering with the formation of bacterial biofilms is the key to blocking subsequent biofouling.

[0004] Marine antifouling functional surfaces currently mainly include traditional toxic antifouling surfaces and new environmentally friendly antifouling surfaces.

[0005] (1) Traditional toxic antifouling surface

[0006] Humans have a long history of fighting against marine biofouling. In 700 BC, the Phoenicians began to use lead to cover the bottom of sailboats to inhibit fouling. Later, toxic substances such as mercury, arsenic, and cuprous oxide were used as antifouling agents to kill fouling organisms. In the 1950s, tributyltin (TBT) was discovered and widely used due to its excellent antifouling ability. Tributyltin has the characteristics of broad spectrum and long-term effect. However, due to its negative impact on the marine environment, the Marine Environment Protection Committee (MEPC) of the International Maritime Organization (IMO) has promulgated regulations in 2008 to prohibit the use of TBT-type surfaces on ship surfaces. Since then, environmentally friendly antifouling surfaces have become a research hotspot.

[0007] (2) Environmentally friendly anti-fouling technology

[0008] Environmentally friendly antifouling surfaces that have emerged in recent years can be roughly divided into the following categories: ① Antifouling surfaces containing natural products, which extract natural products with antifouling activity from marine organisms (mainly algae, seaweed, marine invertebrates and microorganisms) and terrestrial organisms (such as peppers), and compound them into other materials to obtain antifouling surfaces. However, biological antifouling strategies are usually diverse, and surfaces containing a single antifouling agent are difficult to achieve broad-spectrum and long-term antifouling properties, and are still limited in actual engineering applications. ② Fouling-release surfaces, fouling organisms have low adhesion on low surface energy surfaces and are easily desorbed from the surface under shear forces such as water flow, playing an antifouling role. However, this type of surface will only be effective under shear forces exceeding a certain hydrodynamic force, which means that the effect will only be significant when applied to high-speed ships, and it will not be very effective for ships in a moored state and facilities such as aquaculture. ③ Conductive antifouling surface: a conductive coating is applied to the surface of the ship, and an electric current is passed to electrolyze seawater to produce hypochlorite ions, thereby preventing the attachment of marine organisms such as bacteria, algae, and shellfish. Although conductive antifouling coatings have excellent potential, their practical application as antifouling technology needs to be further deepened. ④ Bionic morphology antifouling surface: by imitating typical biological surfaces (such as sharks, lotus leaves, etc.), advanced manufacturing technologies (such as reactive ion beam etching, plasma etching, laser processing, nanoimprint lithography, electrospinning, electrochemical deposition, etc.) are used to construct a single-level or multi-level topological bionic micro-nanostructure surface. The antifouling effect is excellent, but there are also certain defects. A typical example is the American Sharklet antifouling surface. Due to its high production cost, its commercial application in the field of ships has failed. Summary of the invention

[0009] In order to solve the above problems, inspired by the dynamic epidermal antifouling structure of typical cetacean skin, the present invention proposes a bionic antifouling surface and a preparation method thereof.

[0010] The technical solution adopted by the present invention is as follows:

[0011] The micro-electric bionic dynamic anti-fouling surface of the present invention is composed of an ion exchange membrane, an electrode material on the surface of the ion exchange membrane, and a low surface energy anti-fouling surface material on the surface of the electrode material. The ion exchange membrane has a porous three-dimensional network structure for absorbing and retaining water, and has softness and elasticity. The electrode material can drive the ion exchange membrane to generate electroosmotic flow under the stimulation of an external electric field and cause the hydrogel material to undergo macroscopic deformation under the electroosmotic action, so that the anti-fouling surface material on the surface of the electrode material produces microscopic fluid flow.

[0012] The ion exchange membrane material described in the present invention is

[0013] A combination of one or more of fluoride ion exchange membranes (such as polytetrafluoroethylene, polyvinylidene fluoride, etc.), sulfonate ion exchange membranes (such as polystyrene sulfonic acid membranes, polyethersulfone sulfonic acid membranes, polyaniline sulfonic acid membranes, polyvinyl alcohol sulfonic acid membranes, polybenzimidazole sulfonic acid membranes, sulfonated polyarylether membranes, etc.), natural polymer ion exchange membranes, composite ion exchange membranes, and non-perfluorinated ion exchange membranes.

[0014] The method for preparing the bionic antifouling surface of the present invention is as follows:

[0015] (1) Preparation of ion exchange membranes;

[0016] The ion exchange membrane is formed by the polymerization reaction of the ion exchange membrane monomer initiated by an initiator under the action of heat, light or chemical substances, and a cross-linking agent is added to form an ion exchange membrane cross-linking network.

[0017] The ion exchange membrane monomer is a combination of one or more of styrene, vinylbenzene, divinylbenzene, methacrylic acid, acrylamide, chloromethylstyrene, dimethylaminoethyl methacrylate, vinylpyridine, acrylic acid, tetrafluoroethylene, perfluorosulfonic acid vinyl ether, perfluoroethylene propylene, propylene oxide, and ethylene oxide.

[0018] The ion exchange membrane initiator is one of ammonium persulfate, azobisisobutyronitrile, potassium persulfate, phenyldiazane, hydrogen peroxide, ultraviolet light initiator, peroxide, infrared light initiator and radiation initiator.

[0019] The ion exchange membrane crosslinking agent is a combination of one or more of divinylbenzene, vinyltrimethylchlorosilane, vinyltrichlorosilane, methyl methacrylate, tetrahydrofuran multifunctional monomer, trimethoxysilane trimethacrylate, isocyanate compounds, epoxy compounds, allyl monomers, and methacrylic acid crosslinking agent.

[0020] (2) Preparation of electrode materials

[0021] Electrode materials are prepared by physical deposition, chemical deposition, conductive polymer coating, nanomaterial composite, deposition of metal film, self-assembled monolayer, 3D printing technology, etc. 3 S cm -1 The prepared electrode can simultaneously achieve high conductivity (>10 3 S cm -1 ) and high mechanical deformability.

[0022] The electrode material is a combination of one or more of metals and their alloys (copper, silver, gold, aluminum, copper, nickel, platinum, palladium, etc.), carbon-based materials (graphite, graphene, carbon nanotubes, conductive carbon black, activated carbon, carbon fiber, etc.), MXenes (Ti3C2, Ti2C, V2C, Nb2C, Mo2C, Ti4N3, Ti2N, etc.), two-dimensional materials (transition metal sulfides, black phosphorus), conductive polymer materials (polyaniline, polypyrrole, polythiophene, etc.), conductive oxides (zinc oxide, iron oxide, indium tin oxide, etc.), metal / carbon composites, conductive polymer composites, perovskite materials, conductive inks, and the like.

[0023] (3) Preparation of low surface energy antifouling layer

[0024] In order to further reduce the possibility of marine organisms adhering to the surface, it is also necessary to construct a low surface energy antifouling layer on the surface of the material. The low surface energy material is introduced into fluorine or silicon groups through coating, chemical grafting, plasma treatment, blending, physical adsorption, nanotechnology, 3D printing, etc. to form a low surface energy antifouling layer on the surface of the electrode material. Among them, chemical grafting is free radical grafting, surface activation or photochemical grafting;

[0025] The low surface energy material is a combination of one or more of fluoropolymers, silicone polymers, polyethylene, polypropylene, polyepoxide, polystyrene, polyurethane, polyetheretherketone, polyvinyl alcohol, polyisobutylene, polymethyl methacrylate, polycarbonate and the like, and a combination of monomers or monomer derivatives of these substances.

[0026] The thickness of the finally prepared bionic antifouling surface is 10 μm to 5000 μm.

[0027] Beneficial effects of the present invention:

[0028] 1. The micro-electric bionic dynamic repellent antifouling surface is constructed based on the electroosmotic effect. Electroosmosis (electroosmotic flow) is a liquid movement phenomenon caused by an electric field. When the solid surface in the solution is charged due to the dissociation of surface groups or the selective adsorption of certain ions from the solution, due to the requirement of electrical neutrality, there must be excess counterions in the liquid near the charged surface with the same number of charges as the solid surface but opposite signs, forming the so-called double layer. When an electric field is applied to such a system, the net charge in the double layer moves under the action of the Coulomb force, causing the liquid to flow. This flow is electroosmotic flow. Under the action of external electrical stimulation, the bionic antifouling surface exhibits reversible macroscopic mechanical deformation and microscopic fluid flow similar to that of cetacean skin. Based on this principle, the present invention provides a new antifouling solution.

[0029] 2. The microscopic fluid flow of the micro-electro-bionic dynamic drive anti-fouling surface can effectively destroy the stable microenvironment for the growth and reproduction of microorganisms, prevent the adhesion of microorganisms on the surface of the material, and play an efficient anti-fouling role in components such as ships, seawater pipelines, marine detection equipment and high-performance marine sports equipment.

[0030] 3. The macroscopic fluid disturbance of the micro-electric bionic dynamic drive away anti-fouling surface can effectively drive away large fouling organisms and prevent them from adhering to the surface.

[0031] 4. The low surface energy antifouling surface greatly reduces the possibility of marine organisms forming biofilms on it by creating an extremely smooth and unfavorable surface for microbial attachment at the microscopic level.

[0032] 5. The micro-electric bionic dynamic anti-fouling surface is constructed based on the ion migration effect, which can achieve excellent material deformation performance and ion migration at low voltage (<3V). When low voltage is applied, these structures can generate tiny electric fields that cause micro-flows of liquid on the surface of the material. This flow helps to push away liquid and suspended particles on the surface, including dirt and microorganisms, thereby preventing them from accumulating on the surface. This process is not only very effective in preventing the attachment of organisms, but also because the voltage used is very low, the energy consumption is extremely low, and it has little effect on the overall energy efficiency of the device.

[0033] 6. This ion migration-driven antifouling mechanism allows for dynamic control of the antifouling effect. By adjusting the applied voltage and current, the intensity of ion migration can be adjusted as needed, thereby optimizing the antifouling performance under different environmental conditions.

[0034] 7. Ability to resist various biological fouling in a purely physical way, such as the attachment of bacteria, algae and other organisms. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of the structure of the bionic antifouling functional surface based on the ion migration effect;

[0036] Figure 2 This is an electron microscope image of an ion exchange membrane;

[0037] Figure 3 This is a physical picture of the ion exchange membrane surface before and after it is covered with metal electrodes;

[0038] Figure 4 This is a physical picture of the deformation of the micro-electric bionic dynamic anti-fouling surface under a voltage of 3V;

[0039] Figure 5 This is a real picture of the reversible flow of liquid on the bionic antifouling functional surface at 3V voltage;

[0040] Figure 6The antifouling performance test of the bionic antifouling functional surface is compared with the PU antifouling coating. DETAILED DESCRIPTION

[0041] In order to further understand the present invention, the preparation method and application of the micro-electric bionic dynamic anti-fouling surface provided by the present invention are described below in conjunction with the embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0042] Example 1

[0043] 1. Preparation of ion exchange membrane

[0044] Nafion / EG membranes were prepared by ethylene glycol (EG) solution casting method: First, Nafion solution was evaporated to dryness at 70°C to obtain solid Nafion resin. Then, the solid Nafion resin was redissolved in EG at 60°C with magnetic stirring for 6 hours. The volume ratio of the initial Nafion solution and EG was 1:9. Subsequently, the Nafion EG solution was treated under vacuum conditions for 10 minutes to remove air bubbles. During this period, two polytetrafluoroethylene (PTFE) plates were polished with 1000-grit sandpaper and washed with deionized water for later use. Then, the Nafion EG solution was poured into a homemade silicone mold (26mm x26mm x 50mm), and the polished PTFE plate was placed at the bottom of the mold. Next, the mold was heated in a vacuum oven at 120°C and a vacuum pressure of -1 bar for a sufficient time to obtain a solid Nafion / EG membrane. The membrane was brown and formed on the PTFE plate at the bottom of the mold. Then, remove the PTFE plate from the mold and press another polished PTFE plate onto the surface of the membrane. After that, clamp the two PTFE plates with a clamp. Subsequently, place the clamp in a vacuum oven and anneal at 200°C for 1 hour. After cooling in the oven for 10 hours, remove the PTFE plate from the clamp and use a knife to peel the solid Nafion / EG membrane from the PTFE plate. The thickness of the Nafion / EG membrane can be adjusted by simply changing the volume of the applied Nafion solution.

[0045] 2. Preparation of Electrodes

[0046] (1) Pretreatment of Nafion / EG membrane.

[0047] First, the membrane was cleaned with deionized water in an ultrasonic bath for 10 minutes. Then, the membrane was immersed in a 0.5wt% hydrogen peroxide (H2O2) solution for 1 hour and boiled in deionized water at 100°C for 2 hours. After that, the membrane was immersed in a 0.5wt% sulfuric acid (H2SO4) solution for 1 hour and then boiled in deionized water at 100°C for 1 hour. Before electrochemical plating, the pretreated membrane was also immersed in a 10wt% Pt(NH3)4Cl2 aqueous solution for 48 hours. During the pretreatment process, hydrogen peroxide was used to remove organic impurities and acid treatment was used to protonate the Nafion membrane. After pretreatment, the color of the membrane changed from brown to transparent and colorless.

[0048] (2) Ethanol-assisted electrochemical plating process.

[0049] First, the membrane was immersed in a vigorously stirred ethanol solution at 40°C. At the same time, 0.5 ml of a 0.5 wt% KBH4 aqueous solution was added to the ethanol solution every 10 minutes, and this was repeated 12 times. It is worth noting that the volume ratio of ethanol to deionized water in the ethanol solution was 1:5 to allow for moderate expansion of the membrane. The entire process of step (2) was repeated twice to ensure that the Pt electrode had good conductivity.

[0050] (3) Ion exchange process.

[0051] First, the membrane with the Pt electrode was vacuum dried at 100°C for 10 minutes. Next, the dried membrane was immersed in deionized water to fully swell again. Finally, the swollen membrane was immersed in a saturated NaCl aqueous solution for 24 hours to allow for sufficient sodium ion exchange.

[0052] 3. Preparation of low surface energy antifouling surfaces

[0053] By a simple dip coating method, bis(3-aminopropyl)-terminated PDMS and benzene-1,3,5-tricarboxaldehyde solution were used to uniformly coat the PDMS containing imine groups on the micro-electro-bionic dynamic repelling antifouling surface to form a PDMS layer of about 10 μm on the bionic antifouling surface.

[0054] Example 2

[0055] 1. Preparation of ion exchange membrane

[0056] First, 10g of polyetheretherketone (PEEK) was dissolved in 150mL of H2SO4 (98wt%) and reacted at 25°C for 2 days to obtain sulfonated PEEK with a sulfonation degree of 60% (DS=60%). Subsequently, the mixture was treated with a 5wt% NaOH aqueous solution and soaked at 25°C for 12 hours, and sulfonated PEEK in the form of sodium sulfonate was obtained after washing and drying. Next, 0.85g of sulfonated PEEK (DS=60%) was weighed and dissolved in 10 ml of N,N-dimethylacetamide. 0.15g of PEEK particles with an average particle size of 1μm were added to this solution, and treated with a high-speed disperser (2000rpm) for 30 minutes to form an N,N-dimethylacetamide slurry of sulfonated PEEK doped with PEEK particles. Then, the slurry was cast into a membrane and dried at 80°C for 12 hours, and then further dried at 120°C in a vacuum environment for 12 hours to obtain a PEEK particle-doped sulfonated PEEK-based composite membrane. Finally, the obtained composite membrane was treated at 360°C in a vacuum state for 30 minutes to form a sulfonated PEEK-based composite ion exchange membrane reinforced by a crystalline PEEK three-dimensional network.

[0057] 2. Preparation of Conductive Electrodes

[0058] A total of 5 g of polydimethylsiloxane (PDMS) precursor and 0.5 g of cross-linking agent were dispersed in 20 g of ethyl acetate solution and stirred at room temperature until completely dissolved. Multi-walled carbon nanotubes with relative masses of 13%, 15% and 17% were added to the above mixture, stirred at room temperature for 1 hour, and then allowed to stand for 0.5 hours by ultrasonic oscillation to obtain a conductive solution. Subsequently, the conductive solution was first sprayed on the ion exchange membrane, paying attention to controlling the spraying distance and number of times, and operating the entire process in a protective cover. After spraying, the composite film was allowed to stand for 10 minutes to avoid rapid evaporation of the organic solvent due to temperature changes. The film was then cured in an oven at 60°C for 2 hours and aged at 100°C for 2 hours. Finally, a conductive ion exchange membrane was successfully obtained using a sputtering current of 30 mA and a sputtering time of 200 seconds.

[0059] 3. Preparation of low surface energy antifouling surfaces

[0060] By a simple dip coating method, bis(3-aminopropyl)-terminated PDMS and benzene-1,3,5-tricarboxaldehyde solution were used to uniformly coat the PDMS containing imine groups on the micro-electro-bionic dynamic repelling antifouling surface to form a PDMS layer of about 10 μm on the bionic antifouling surface.

[0061] In the process of preparing the ion exchange membrane, by changing one or more combinations of reaction conditions such as temperature, pressure, pH value, type and concentration of initiator, type and concentration of cross-linking agent, post-treatment of the ion exchange membrane, or by adding specific chemical substances, the water absorption rate and expansion behavior, mechanical properties, pore structure and pore size distribution, chemical stability, network structure and cross-linking density, and responsiveness of the ion exchange membrane can be regulated. By adjusting one or more combinations of parameters such as temperature, pressure, humidity, chemical environment, preparation time, etc. during the preparation process, a surface electrode with good conductivity, flexibility, mechanical properties, and strong bonding strength with the ion exchange membrane substrate is obtained.

[0062] During the preparation of the electrode, by adjusting one or more combinations of parameters such as temperature, pressure, humidity, chemical environment, preparation time, etc. during the preparation process, a surface electrode with good conductivity, flexibility, mechanical properties and strong bonding strength with the hydrogel matrix is ​​obtained.

[0063] Effect verification:

[0064] like Figure 1 The figure shows the schematic diagram of the structure of the bionic antifouling functional surface based on the electroosmotic effect; Figure 4 As shown in the figure, after applying 3V direct current to the electrodes on both sides, the liquid (seawater) in the ion exchange membrane will form a double layer, and the net charge in the double layer will move due to the Coulomb force of the electric field. At the same time, due to the solvation effect, the movement of the charge will drive the flow of the liquid around the charge, which will lead to the flow of the liquid in the ion exchange membrane to form electroosmotic flow. On a macro scale, the flow of liquid will cause the volume of the hydrogel to expand / contract, thereby causing the hydrogel to deform. Figure 5 The figure shows the reversible electroosmotic effect of the bionic antifouling functional surface at 3V. The surface has undergone significant shape changes from before to after. The bionic antifouling surface sample and the polyurethane (PU) coating surface were subjected to antibacterial experiments. Figure 6 The bacteria removal rate shown was over 97.5%.

[0065] It can be seen that when voltage is applied to the electrode, current begins to flow through the metal electrode. This current causes the migration of cations and water molecules in the ion exchange membrane. These ions and water molecules move from one electrode to another. At this time, one side of the ion exchange membrane begins to expand, while the other side begins to shrink. This drives the ion exchange membrane to undergo macroscopic deformation. When the positive and negative directions of the power supply are changed, the movement direction of the ions and water molecules will change. By continuously switching the positive and negative poles of the power supply and adjusting the switching frequency, the degree, direction and speed of deformation of the material can be precisely controlled. This further regulates the macroscopic disturbance of the bionic antifouling surface. In addition, when ions and water molecules move from one electrode to another, a reversible flow of liquid inside and outside the pores of the bionic antifouling surface will occur. The reversible flow of the liquid will disturb the liquid around the bionic antifouling surface, thereby preventing the adhesion of fouling organisms.

Claims

1. A micro-electric bionic dynamic anti-fouling surface, characterized in that: The antifouling surface is composed of an ion exchange membrane, an electrode material on the surface of the ion exchange membrane, and a low surface energy antifouling surface layer material on the surface of the electrode material; The ion exchange membrane has a porous three-dimensional network structure for absorbing and retaining water, and has softness and elasticity; the electrode material can drive the ion exchange membrane to generate electroosmotic flow under the stimulation of an external electric field and cause the hydrogel material to undergo macroscopic deformation under the electroosmotic action, causing the antifouling surface material on the surface of the electrode material to produce microscopic fluid flow; The ion exchange membrane material is a combination of one or more of a fluoride ion exchange membrane, a sulfonate ion exchange membrane, a natural polymer ion exchange membrane, a composite ion exchange membrane, and a non-perfluorinated ion exchange membrane.

2. The micro-electric bionic dynamic anti-fouling surface according to claim 1 is characterized in that: The fluoride ion exchange membrane is a polytetrafluoroethylene or polyvinylidene fluoride ion exchange membrane; The sulfonated ion exchange membrane is a polystyrene sulfonic acid membrane, a polyethersulfone sulfonic acid membrane, a polyaniline sulfonic acid membrane, a polyvinyl alcohol sulfonic acid membrane, a polybenzimidazole sulfonic acid membrane or a sulfonated polyarylether membrane.

3. The micro-electric bionic dynamic anti-fouling surface according to claim 1 is characterized in that: The low surface energy material is a combination of one or more of fluoropolymer, silicon polymer, polyethylene, polypropylene, polyepoxide, polystyrene, polyurethane, polyetheretherketone, polyvinyl alcohol, polyisobutylene, polymethyl methacrylate, and polycarbonate.

4. The micro-electric bionic dynamic anti-fouling surface according to claim 1, characterized in that: The electrode material is a combination of one or more of metals and their alloys, carbon-based materials, MXenes, transition metal sulfides, black phosphorus, conductive polymer materials, conductive oxides, metal / carbon composites, conductive polymer composites, perovskite materials, and conductive inks.

5. The micro-electric bionic dynamic anti-fouling surface according to claim 4 is characterized in that: The metal is copper, silver, gold, aluminum, copper, nickel, platinum or palladium; the carbon-based material is graphite, graphene, carbon nanotubes, conductive carbon black, activated carbon or carbon fiber; MXenes are Ti3C2, Ti2C, V2C, Nb2C, Mo2C, Ti4N3 or Ti2N; the conductive polymer material is polyaniline, polypyrrole or polythiophene; the conductive oxide is zinc oxide, iron oxide or indium tin oxide.

6. The method for preparing a micro-electric bionic dynamic anti-fouling surface as claimed in claim 1, characterized in that: The steps of this method are as follows: (1) Preparation of ion exchange membrane The ion exchange membrane is formed by the polymerization reaction of the ion exchange membrane monomer initiated by an initiator under the action of heat, light or chemical substances, and a cross-linking agent is added to form an ion exchange membrane cross-linking network. (2) Preparation of electrode materials The electrode material is prepared by one of the methods such as physical deposition, chemical deposition, conductive polymer coating, nanomaterial composite, deposition of metal film, self-assembled monolayer, 3D printing technology, etc.; (3) Preparation of low surface energy antifouling layer A low surface energy antifouling layer is formed on the surface of the electrode material by introducing fluorine or silicon groups into the low surface energy material through coating, chemical grafting, plasma treatment, blending, physical adsorption, nanotechnology, and 3D printing. Among them, the chemical grafting is free radical grafting, surface activation or photochemical grafting.

7. The method for preparing a micro-electric bionic dynamic anti-fouling surface according to claim 6, characterized in that: The ion exchange membrane monomer is a combination of one or more of styrene, vinylbenzene, divinylbenzene, methacrylic acid, acrylamide, chloromethylstyrene, dimethylaminoethyl methacrylate, vinylpyridine, acrylic acid, tetrafluoroethylene, perfluorosulfonic acid vinyl ether, perfluoroethylene propylene, propylene oxide, and ethylene oxide.

8. The method for preparing a micro-electric bionic dynamic anti-fouling surface according to claim 6, characterized in that: The ion exchange membrane initiator is one of ammonium persulfate, azobisisobutyronitrile, potassium persulfate, phenyldiazane, hydrogen peroxide, ultraviolet light initiator, peroxide, infrared light initiator and radiation initiator.

9. The method for preparing a micro-electric bionic dynamic anti-fouling surface according to claim 6, characterized in that: The ion exchange membrane crosslinking agent is a combination of one or more of divinylbenzene, vinyltrimethylchlorosilane, vinyltrichlorosilane, methyl methacrylate, tetrahydrofuran multifunctional monomer, trimethoxysilane trimethacrylate, isocyanate compounds, epoxy compounds, allyl monomers, and methacrylic acid crosslinking agent.