Asphalt flame retardant, flame-retardant asphalt and preparation method of flame-retardant asphalt
By using a mixture of hydroxide, eloite nanotubes and ferrocene as flame retardant in asphalt, combined with synergistic agent and high-speed shearing process, traditional asphalt flammable and high hydroxide dosage is solved. The problem is that efficient flame retardant and smoke suppression effects are achieved, while improving the rheological performance and high temperature stability of asphalt.
Patent Information
- Application Number
- CN202411359536.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional road asphalt is flammable under high temperature conditions, and releases toxic and harmful gases during combustion, which increases the risk of fire accidents. The commonly used hydroxide flame retardant requires a large amount to produce effects, which weakens the rheological performance of asphalt and Economic benefits.
Use a mixture of 60% to 90% hydroxide and 10% to 40% eloite nanotubes and ferrocene as the asphalt flame retardant, and combine it with 0 to 5% synergistic agents, such as montmorillonite, oxidation Antimony and its derivatives, zinc borates, and organotin compounds are prepared by heating and high-speed shearing processes.
It significantly improves the flame retardant and smoke suppression properties of asphalt, enhances rheology performance and high temperature stability, has simple process, low ingredients and strong economic benefits.
Smart Images

Figure CN118956003A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of flame retardants, and in particular to an asphalt flame retardant, flame retardant asphalt and a preparation method thereof. Background Art
[0002] In the construction of modern transportation infrastructure, tunnels are important transportation channels, and their safety and durability have received widespread attention. The internal environment of tunnels is complex and the space is relatively closed. Once a fire occurs, it will greatly threaten the safety of personnel and the integrity of the tunnel structure. Traditional road asphalt is flammable under high temperature conditions, and a large amount of toxic and harmful gases will be released during the combustion process, greatly increasing the risk and consequences of fire accidents. In recent years, with the development of materials science, flame retardant asphalt has emerged and has shown good application prospects.
[0003] However, the flame retardancy requirements of general asphalt are achieved through flame retardants. The common type of flame retardant in asphalt is hydroxide, which is widely used due to its non-toxicity, environmental protection and low cost. However, hydroxide requires a large dosage to produce an effect, which often weakens the rheological properties and economic benefits of asphalt. Summary of the invention
[0004] In view of the above problems, the present invention aims to provide an asphalt flame retardant, a flame retardant asphalt and a preparation method thereof.
[0005] The technical solution of the present invention is as follows:
[0006] On the one hand, an asphalt flame retardant is provided, which comprises, by mass percentage, 60% to 90% of a hydroxide and 10% to 40% of a mixture of halloysite nanotubes and ferrocene, and the mass ratio of the halloysite nanotubes to the ferrocene in the mixture is 1:2 to 2:1.
[0007] Preferably, the mixture comprises 80% of hydroxide and 20% of halloysite nanotubes and ferrocene, and the mass ratio of the halloysite nanotubes to the ferrocene in the mixture is 1:1.
[0008] Preferably, the hydroxide is any one or more of aluminum hydroxide, magnesium hydroxide and calcium hydroxide.
[0009] On the other hand, a flame retardant asphalt is also provided, which comprises, by mass percentage, 85% to 90% of asphalt, 0 to 5% of a synergist and 10% of an asphalt flame retardant, and the asphalt flame retardant is any one of the asphalt flame retardants described above.
[0010] Preferably, the synergist is any one or more of montmorillonite, antimony oxide and its derivatives, zinc borate, and organic tin compounds.
[0011] On the other hand, a method for preparing the flame retardant asphalt described in any one of the above is also provided, comprising the following steps:
[0012] S1: heating the asphalt to change the asphalt from solid to liquid to obtain liquid asphalt;
[0013] S2: adding the synergist and the asphalt flame retardant to the liquid asphalt, stirring for 5 to 10 minutes, to obtain a mixed asphalt;
[0014] S3: sending the mixed asphalt into a high-speed shearing device for shearing to remove bubbles and obtain the flame-retardant asphalt.
[0015] Preferably, in step S1, heating is performed at 170°C.
[0016] Preferably, in step S3, when shearing is performed, shearing is first performed at 3000-4000 r / min for 30-50 min, and then shearing is performed at 500 r / min for 5-10 min.
[0017] Preferably, during shearing, the material is first sheared at 3500 r / min for 30 min, and then sheared at 500 r / min for 5 min.
[0018] Preferably, when shearing is performed, shearing is first performed at 4000 r / min for 30 min, and then shearing is performed at 500 r / min for 5 min.
[0019] The beneficial effects of the present invention are:
[0020] (1) Compared with other flame retardant products, the asphalt flame retardant of the present invention can significantly improve the flame retardancy and smoke suppression properties of asphalt.
[0021] (2) The flame retardant asphalt preparation process of the present invention is simple and is conducive to practical engineering applications.
[0022] (3) Each component of the asphalt flame retardant of the present invention is low in price and has strong economic benefits.
[0023] (4) The asphalt flame retardant of the present invention can improve the rheological properties and high temperature stability of asphalt in addition to improving the flame retardancy and smoke suppression properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0025] Figure 1 This is a schematic diagram of the comparison results of smoke density levels of different asphalt flame retardants;
[0026] Figure 2 This is a schematic diagram of the comparison of oxygen indexes of different asphalt flame retardants;
[0027] Figure 3 Schematic diagram of cone calorimetry results for different asphalt flame retardants; Figure 3 (a) is a schematic diagram of the heat release peak. Figure 3 (b) is a schematic diagram of total heat release. Figure 3 (c) is a schematic diagram of the peak smoke release. Figure 3 (d) is a schematic diagram of total smoke release;
[0028] Figure 4 Schematic diagram of DSR comparison results of different asphalt flame retardants; Figure 4 (a) is a schematic diagram of the relationship between complex shear modulus and temperature. Figure 4 (b) is a schematic diagram of the relationship between phase angle and temperature. Figure 4 (c) is a schematic diagram of the relationship between rutting factor and temperature. Figure 4 (d) is a schematic diagram showing the relationship between failure temperature and material type;
[0029] Figure 5 It is a schematic diagram of the oxygen index results of the asphalt flame retardant of the present invention and different warm mix agents;
[0030] Figure 6 It is a schematic diagram of cone calorimetry results of the asphalt flame retardant of the present invention and different warm mix agents; Figure 6 In the embodiment, F is the asphalt flame retardant of Example 8 of the present invention, S, E, and M are organic warm mixing agent, chemical warm mixing agent, and foaming warm mixing agent, respectively. DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with the accompanying drawings and embodiments. It should be noted that, in the absence of conflict, the embodiments in this application and the technical features in the embodiments can be combined with each other. It should be noted that, unless otherwise specified, all technical and scientific terms used in this application have the same meanings as those generally understood by those of ordinary skill in the art to which this application belongs. The words "including" or "comprising" and the like used in the disclosure of the present invention mean that the elements or objects appearing before the word cover the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0032] On the one hand, the present invention provides an asphalt flame retardant, which comprises, by mass percentage, 60% to 90% of a hydroxide and 10% to 40% of a mixture of halloysite nanotubes and ferrocene, and the mass ratio of the halloysite nanotubes to the ferrocene in the mixture is 1:2 to 2:1.
[0033] In a specific embodiment, the asphalt flame retardant includes 80% of hydroxide and 20% of a mixture of halloysite nanotubes and ferrocene, and the mass ratio of the halloysite nanotubes to the ferrocene in the mixture is 1:1.
[0034] In a specific embodiment, the hydroxide is any one or more of aluminum hydroxide, magnesium hydroxide, and calcium hydroxide. Optionally, the hydroxide is a mixture of aluminum hydroxide and magnesium hydroxide, and the ratio of the two is 1:1 to 1:2. It should be noted that in addition to the hydroxide combination selected in this embodiment, other combinations and other hydroxides may also be applicable to the present invention.
[0035] On the other hand, the present invention also provides a flame retardant asphalt, which comprises, by mass percentage, 85% to 90% of asphalt, 0 to 5% of a synergist and 10% of an asphalt flame retardant, and the asphalt flame retardant is any one of the asphalt flame retardants described above.
[0036] In a specific embodiment, the synergist is any one or more of montmorillonite, antimony oxide and its derivatives, zinc borate, and organotin compounds. Optionally, the synergist is zinc borate. It should be noted that the role of the synergist is to reduce the cost while maintaining product performance. In addition to the preferred synergist of this embodiment, other agents that can achieve the same effect may also be applicable to the present invention.
[0037] On the other hand, the present invention also provides a method for preparing the flame retardant asphalt described above, comprising the following steps:
[0038] S1: heating the asphalt to change the asphalt from solid to liquid to obtain liquid asphalt.
[0039] In a specific embodiment, the heating is performed at 170°C.
[0040] S2: adding the synergist and the asphalt flame retardant to the liquid asphalt, stirring for 5 to 10 minutes, and obtaining a mixed asphalt.
[0041] S3: sending the mixed asphalt into a high-speed shearing device for shearing to remove bubbles and obtain the flame-retardant asphalt.
[0042] In a specific embodiment, when shearing is performed, the material is first sheared at 3000-4000 r / min for 30-50 min, and then sheared at 500 r / min for 5-10 min.
[0043] Optionally, when shearing is performed, shearing is first performed at 3500 r / min for 30 min, and then shearing is performed at 500 r / min for 5 min.
[0044] Optionally, when shearing is performed, shearing is first performed at 4000 r / min for 30 min, and then shearing is performed at 500 r / min for 5 min.
[0045] It should be noted that the shearing time and shearing rate in the above-mentioned embodiments are only preferred shearing conditions of the present invention.
[0046] When using the present invention, the average method and the maximum value method can be used together to evaluate the most suitable combination of shear time and shear rate.
[0047] The average value method is to calculate the root mean square average value of the oxygen content of the groups with the same shear time and shear rate, and select the shear time and shear rate with the highest oxygen content;
[0048] The maximum value method refers to selecting the group with the highest oxygen content among all groups and recording its combination.
[0049] In a specific embodiment, a flame retardant asphalt is prepared by the following steps:
[0050] (1) heating 90 parts of asphalt in an oil bath to about 170° C. to change the asphalt from solid to liquid, thereby obtaining liquid asphalt;
[0051] (2) adding 10 parts of an asphalt flame retardant consisting of hydroxide, halloysite nanotubes, and ferrocene to the liquid asphalt, stirring for 5 to 10 minutes, and obtaining a mixed asphalt;
[0052] (3) The mixed asphalt is sent to a high-speed shearing device for shearing to remove bubbles and obtain the flame-retardant asphalt.
[0053] In the above embodiments, flame retardant asphalt of multiple embodiments is obtained by changing the dosage of each agent of the asphalt flame retardant in step (2) and the high-speed shear time and shear rate in step (3).
[0054] The parameter design and oxygen index test results of the flame retardant asphalt in each embodiment are shown in Table 1:
[0055] Table 1 Parameter design and oxygen index test results of flame retardant asphalt in various embodiments
[0056]
[0057] In addition to the above-mentioned embodiments, asphalt flame retardants with the following proportions were obtained by changing the composition formula of the asphalt flame retardant and were tested experimentally.
[0058] The relevant parameter design and oxygen index test results are shown in Table 2:
[0059] Table 2 Comparative example parameters and oxygen index test results of flame retardant asphalt in each comparative example
[0060]
[0061] The national standard GB29051 stipulates that the oxygen index (an indicator for evaluating the ignition difficulty of a material) of asphalt used in tunnel roads should not be less than 23%.
[0062] It can be seen from Table 1 that the flame retardant asphalt of the present invention can meet the requirements. When the hydroxide content is 8%, the halloysite nanotube content is 1%, and the ferrocene content is 1%, the oxygen index is as high as 28.1%.
[0063] By comparing Table 1 and Table 2, it can be seen that, when the hydroxide content is the same, the oxygen index of the flame retardant asphalt to which only halloysite nanotubes or only ferrocene are added is not as high as the oxygen index of the flame retardant asphalt of the present invention; the oxygen index of the flame retardant asphalt to which only halloysite nanotubes or ferrocene are added without adding hydroxide cannot meet the requirements.
[0064] In addition, the smoke density and oxygen index of the product of the present invention in Example 8 above were compared with asphalt, flame retardant asphalt with commercial flame retardant 1 added, and flame retardant asphalt with commercial flame retardant 2 added. The results are as follows: Figures 1-2 As shown. Figures 1-2 It can be seen that the product of the present invention can significantly reduce the smoke density level of asphalt and improve the oxygen index. Compared with existing commercial flame retardants, the improvement effect is more obvious.
[0065] The product of the present invention in Example 8 was tested with a cone calorimeter, asphalt, flame retardant asphalt with commercial flame retardant 1, and flame retardant asphalt with commercial flame retardant 2. The test results were: Figure 3 As shown. Figure 3 It can be seen that compared with commercial flame retardants and pure asphalt, the peak heat release, total heat release, peak smoke release and total smoke release of the present invention are greatly reduced.
[0066] The product of the present invention in Example 8 and asphalt, flame retardant asphalt with commercial flame retardant 1, and flame retardant asphalt with commercial flame retardant 2 were subjected to a dynamic shear rheometer (DSR) test of asphalt. The results are as follows: Figure 4 As shown. DSR is a common test method used to evaluate the viscoelastic properties of asphalt materials under different temperature and stress conditions. The DSR test is mainly used to analyze the rutting resistance, fatigue resistance, and high and low temperature performance of asphalt materials, especially in road construction and material development. The failure temperature refers to the temperature at which asphalt loses sufficient resistance to deformation under high temperature conditions. Usually, the failure temperature is used to evaluate the high temperature rutting resistance of asphalt, that is, the stability of asphalt under high temperature conditions in road paving materials.
[0067] Figure 4 The complex shear modulus represents the ability of asphalt to resist shear deformation. The larger the value at the same temperature, the stronger the ability to resist shear deformation. The phase angle represents the ratio between the viscosity and elasticity of asphalt. The larger the value at the same temperature, the greater the viscosity component of the asphalt and the larger the irrecoverable deformation portion. Therefore, the smaller the value, the stronger the asphalt's ability to resist deformation. The rutting factor is a comprehensive evaluation index of asphalt's high-temperature stability. The larger the value at the same temperature, the stronger the ability to resist shear rheological deformation and the better the high-temperature stability. The failure temperature represents the temperature at which asphalt loses its function at high temperatures. The higher the value, the better the high-temperature rheological properties of the asphalt. Figure 4 It can be seen that the rheological properties of the present invention in asphalt are higher than those of traditional commercial flame retardants; the present invention can improve the high-temperature stability of asphalt; and compared with commercial flame retardants, the improvement effect of the present invention is more obvious. The failure temperature of ordinary asphalt is around 75°C, and after the commercial flame retardant is added to asphalt, the failure temperature of asphalt is increased to 80-85°C. When this product is added to asphalt, the failure temperature of asphalt reaches 94°C, which greatly improves the high-temperature performance of asphalt.
[0068] In addition, the current tunnel asphalt is mostly warm mix asphalt, with warm mix agent added. In order to meet the mainstream application scenarios, the effects of the product of the present invention and the warm mix agent are further tested.
[0069] Currently, there are three types of warm mix agents: organic, chemical, and foaming. The mechanisms of warm mix agents are different. After testing, the product of the present invention is more suitable for organic warm mix agents (the oxygen index of asphalt + organic warm mix agent is 20.5%, the oxygen index of asphalt + chemical warm mix agent is 19.5%, and the oxygen index of asphalt + bubble warm mix agent is 19.3%). Adding the asphalt flame retardant product of the present invention together with the organic warm mix agent to asphalt (double-modified asphalt) can further improve the flame retardant performance on the basis of single addition. The results are as follows: Figure 5 and Figure 6 shown.
[0070] In summary, the present invention can significantly improve the flame retardancy and smoke suppression performance of asphalt, and at the same time can improve the rheological properties and high temperature stability of asphalt. Compared with the prior art, the present invention has significant progress.
[0071] The above description is only a representative embodiment of the present invention and does not limit the present invention in any form. Any technician familiar with the profession, without departing from the scope of the technical solution of the present invention, uses the above-disclosed technical contents to make some changes or modifications to the embodiments are equivalent embodiments of the present invention. However, any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. An asphalt flame retardant, characterized in that: The invention comprises, by mass percentage, a mixture of 60% to 90% of hydroxide and 10% to 40% of halloysite nanotubes and ferrocene, wherein the mass ratio of the halloysite nanotubes to the ferrocene in the mixture is 1:2 to 2:
1.
2. The asphalt flame retardant according to claim 1, characterized in that: The invention comprises a mixture of 80% hydroxide and 20% halloysite nanotubes and ferrocene, wherein the mass ratio of the halloysite nanotubes to the ferrocene in the mixture is 1:
1.
3. The asphalt flame retardant according to claim 1 or 2, characterized in that: The hydroxide is any one or more of aluminum hydroxide, magnesium hydroxide and calcium hydroxide.
4. A flame retardant asphalt, characterized in that: In terms of mass percentage, it comprises 85% to 90% of asphalt, 0 to 5% of a synergist and 10% of an asphalt flame retardant, and the asphalt flame retardant is the asphalt flame retardant described in any one of claims 1 to 3.
5. The flame retardant asphalt according to claim 4, characterized in that: The synergist is any one or more of montmorillonite, antimony oxide and its derivatives, zinc borate, and organic tin compounds.
6. The method for preparing the flame retardant asphalt according to claim 4 or 5, characterized in that: The following steps are involved: S1: heating the asphalt to change the asphalt from solid to liquid to obtain liquid asphalt; S2: adding the synergist and the asphalt flame retardant to the liquid asphalt, stirring for 5 to 10 minutes, to obtain a mixed asphalt; S3: sending the mixed asphalt into a high-speed shearing device for shearing to remove bubbles and obtain the flame-retardant asphalt.
7. The method for preparing flame retardant asphalt according to claim 6, characterized in that: In step S1, heating is performed at 170°C.
8. The method for preparing flame retardant asphalt according to claim 6, characterized in that: In step S3, when shearing is performed, shearing is first performed at 3000-4000 r / min for 30-50 min, and then shearing is performed at 500 r / min for 5-10 min.
9. The method for preparing flame retardant asphalt according to claim 8, characterized in that: When shearing, first shear at 3500r / min for 30min, and then shear at 500r / min for 5min.
10. The method for preparing flame retardant asphalt according to claim 8, characterized in that: When shearing, first shear at 4000r / min for 30min, and then shear at 500r / min for 5min.