Long light-storing material, preparation method thereof and extrusion equipment for preparing long light-storing material
By using plastic resin, photothermal aging agent, photothermal aging agent and liquid transport agent in long light storage materials, combined with ultrasonic dispersion and liquid metering conveying pump technology, the blackening problem caused by friction between luminous powder and metal is solved, and the problem of blackening caused by friction between luminous powder and metal is achieved. High brightness and long glow time effects.
Patent Information
- Application Number
- CN202411042831.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the molding process, existing long light storage materials are prone to blackening due to friction between luminous powder and metal, which affects the appearance and luminous brightness of the product.
Using a combination of plastic resin, photothermal aging agent, photoacid powder and liquid conveying agent, the photoacid powder is dispersed by ultrasonic wave and pumped into the liquid metering conveying pump to reduce friction with the metal wall, and use a full conveying block Threaded elements and vacuum devices reduce shear friction.
The prepared long-light storage material does not turn black, has high luminous intensity, long luminous time, and has more than 12 hours in dark environments, avoiding blackening and shear damage caused by metal friction.
Smart Images

Figure HDA0004972792390000011 
Figure HDA0004972792390000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of long-duration light-storage materials, and in particular relates to a long-duration light-storage material and a preparation method thereof, and extrusion equipment for preparing the long-duration light-storage material. Background Art
[0002] Long-lasting light-storage materials are also called photoluminescent ultra-long afterglow light-storage materials, non-radioactive light-storage materials, self-luminous materials without power supply, etc. After absorbing visible light such as sunlight, lamplight, stray light, etc., this material can emit a long-lasting high-brightness afterglow in the dark. It has developed rapidly in recent years. However, the hardness of light-storage powder is high, and it will turn black when rubbed with metal, which will affect the appearance of the product and reduce the brightness and time of the product.
[0003] CN1073598C "Nighttime Luminous Plastic Material" discloses that plastic resin and luminous powder are directly mixed and molded; CN104945738A "A Luminous Bumper Plastic" discloses that polypropylene is directly mixed and injected with luminous powder; CN101982501A "Luminous Nylon Material for Injection Molding" discloses that nylon is directly mixed with luminous powder and extruded by a twin screw. However, these technologies all have the problem of friction between the luminous powder and the metal wall during molding, so there is a risk of blackening.
[0004] CN103509363B "A method for preparing luminous plastic injection molding parts" discloses that plastic resin and luminous powder are directly mixed and injection molded, but polytetrafluoroethylene coating is applied to the mold and screw to avoid contact and friction between the luminous powder and metal. CN100547017C "A method for preparing luminous thermoplastic masterbatch", CN116120599A "A luminous plastic particle, a luminous plastic masterbatch containing the same, and a preparation method and application" and CN104059274A "A high-performance light-storing luminous masterbatch for polyolefin plastics and a preparation method" respectively disclose that luminous powder is made into masterbatch to reduce contact and friction between the luminous powder and metal materials. CN107815018B "A luminous plastic, a twin-screw extruder for preparing luminous plastic and a preparation method thereof" discloses that a side feeding device is designed to reduce the residence time of the luminous powder and reduce contact and friction with metal. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a long light-storage material which does not turn black or dark and has high brightness and a long light-emitting time.
[0006] On one hand, the present invention provides a long light-storage material, which is prepared from the following components in parts by weight: 74-97.2 parts of plastic resin, 0.5-1 parts of light-heat aging protection agent, 2-20 parts of light-storage powder, and 0.3-5 parts of liquid delivery agent.
[0007] The plastic resin can be any plastic resin suitable as a matrix of a long light storage material in the art, without particular limitation. For example, the plastic resin can be selected from: polyolefin resins, such as polyethylene (PE), polypropylene (PP), polystyrene (PS), acrylonitrile-butadiene-styrene copolymer (ABS), ethylene / vinyl acetate copolymer (EVA), polyvinyl chloride (PVC); polyurethane (PU) resin; acrylic (PA) resin, such as polymethyl methacrylate (PMMA); epoxy resin; polyester resin, such as polyethylene terephthalate (PET); polycarbonate (PC) resin; polyvinyl butyral resin, etc., but not limited thereto. In particular, the plastic resin can be selected from: PE, PP, ABS, PA6.
[0008] The light and heat aging inhibitor can inhibit oxidation, heat or light, thereby extending the service life of the product. The light and heat aging inhibitor includes a heat aging inhibitor and a light aging inhibitor. For example, the heat aging inhibitor is selected from antioxidant 1010, antioxidant 1076, antioxidant 1098, and antioxidant 168, but is not limited thereto; the light aging inhibitor is selected from light stabilizer 770, UV3853PP5, light stabilizer UV-P, ultraviolet absorber UV-3808, light stabilizer 3346, and light stabilizer 1164, but is not limited thereto.
[0009] The luminescent powder may also be called photoluminescent luminous powder, or photoluminescent material, and may be any luminescent powder known in the art without particular limitation. For example, the luminescent powder may be rare earth sulfide luminescent powder, rare earth aluminate luminescent powder, rare earth silicate luminescent powder, rare earth oxide luminescent powder, rare earth phosphate luminescent powder or a combination thereof.
[0010] Preferably, the molecular formula of the luminescent powder is SrAl2O4:Eu~(2+),Dy~(3+), and the components by weight percentage are 50-60% strontium carbonate, 35-45% aluminum oxide, 1-3% dysprosium oxide, and 1-2% europium oxide.
[0011] The liquid conveying agent is used to disperse the luminescent powder to avoid agglomeration of the luminescent powder, and helps to add the luminescent powder into the processing equipment in a liquid form, which is beneficial to control the addition of the luminescent powder and facilitate the dispersion of the luminescent powder in the resin, reduce the friction between the luminescent powder and the metal wall, and avoid the blackening of the metal due to friction.
[0012] The liquid delivery agent can be selected from diffusion oil Wacker Ak-1000, silane coupling agent KH550, KH560, KH792.
[0013] In some embodiments, the plastic resin is PE, the liquid delivery agent is selected from the diffusion oil Wacker Ak-1000, one of the silane coupling agents KH550, KH560, and KH792, and the light and heat aging protection agent is antioxidant 1010: antioxidant 168: UV3853PP5: 3346 = 0.1-0.3: 0.1-0.3: 0.2-0.4: 02-0.4.
[0014] In some embodiments, the plastic resin is PP, the liquid delivery agent is selected from diffusion oil Wacker Ak-1000, one of silane coupling agents KH550, KH560, and KH792, and the anti-light and heat aging agent is antioxidant 1010: antioxidant 168: ultraviolet absorber UV-3808 = 0.1-0.4: 0.1-0.4: 0.2-0.8.
[0015] In some embodiments, the plastic resin is ABS, the liquid delivery agent is selected from the diffusion oil Wacker Ak-1000, one of the silane coupling agents KH550, KH560, and KH792, and the anti-light and heat aging agent is antioxidant 1076: antioxidant 168: light stabilizer 770: light stabilizer UV-P=0.1-0.3:0.1-0.3:0.2-0.4:02-0.4.
[0016] In some embodiments, the plastic resin is PA6, the liquid delivery agent is selected from the diffusion oil Wacker Ak-1000, one of the silane coupling agents KH550, KH560, and KH792, and the anti-light and heat aging agent is antioxidant 1098: antioxidant 168: light stabilizer 3346: light stabilizer 1164 = 0.1-0.3: 0.1-0.3: 0.2-0.4: 0.2-0.4.
[0017] The second aspect of the present invention provides a method for preparing the long light-storage material, the method is carried out in a twin-screw extruder, the top of the barrel of the twin-screw is provided with a through channel, the through channel is connected to a liquid metering delivery pump with a heating device, the distance between the pump inlet and the die head is 20-100 cm, and the screw thread elements from the pump inlet to the die head are all delivery elements; a vacuum device is provided between the pump inlet and the die head, the distance from the die head is 40-50 cm, and the method comprises the following steps:
[0018] Plastic resin and anti-light and heat aging agent are added from the main feeding port and heated and melted by a twin-screw extruder; the luminescent powder is first dispersed in a liquid conveying agent by ultrasonic wave, and then pumped into the extruder barrel through the top of the barrel by a liquid metering delivery pump to mix with the molten plastic and extrude through a die head, cool, and pelletize.
[0019] According to the method of the present invention, the luminescent powder dispersed in the liquid conveying agent is pumped into the twin-screw extruder and then wrapped by the molten plastic. The residence time in the twin-screw extruder is shorter and there is basically no friction with the metal wall, thus avoiding the blackening of the metal due to friction. In addition, in the present invention, all the screw thread elements between the pump inlet and the die head are conveying elements, which can further reduce the blackening of the luminescent powder due to shearing of the screw.
[0020] In some embodiments, the ultrasonic dispersion time can be determined according to the amount of luminescent powder and liquid delivery agent used and the power of the ultrasonic equipment, as long as the luminescent powder can be evenly dispersed in the liquid delivery agent. For example, the ultrasonic dispersion time can be 0.2-10 min, such as 1-10 min.
[0021] In some embodiments, the temperature of the liquid metering delivery pump is set to 20-60°C.
[0022] In some embodiments, the plastic resin is PE, the extrusion temperature is 160-200° C., and the vacuum degree is ≤-0.08 MPa.
[0023] In some embodiments, the plastic resin is PP, the extrusion temperature is 180-220° C., and the vacuum degree is ≤-0.08 MPa.
[0024] In some embodiments, the plastic resin is ABS, the extrusion temperature is 220-240° C., and the vacuum degree is ≤-0.08 MPa.
[0025] In some embodiments, the plastic resin is PA6, the extrusion temperature is 220-240° C., and the vacuum degree is ≤-0.08 MPa.
[0026] In some embodiments, the through-channel has a diameter of 3-10 mm.
[0027] In some embodiments, the pump inlet is 50-100 cm away from the die.
[0028] The third aspect of the present invention provides an extrusion device for preparing the long light-storage material, which is a twin-screw extruder, characterized in that a through channel is opened at the top of the barrel, and the through channel is connected to a liquid metering delivery pump with a heating device. The pump inlet is 20-100 cm away from the die head, and all the screw thread elements from the pump inlet to the die head are delivery elements; a vacuum device is provided between the pump inlet and the die head, and the distance from the die head to the vacuum device is 40-50 cm.
[0029] Except for the above-mentioned features, the configuration of the extrusion apparatus for preparing the long light storage material according to the present invention is the same as that of a conventional twin-screw extruder.
[0030] Figure 1The main view of the twin-screw extruder connected to the pump inlet barrel of the present invention is shown Figure 1 a, left view Figure 1 b, and overlooking Figure 1 c. As shown in the figure, the cylinder 1 has a positioning pin 4, a cylinder connecting bolt hole 6 and a cylinder inner cavity 2, the cylinder inner cavity 2 has an alloy bushing 3, a through channel is opened on the top of the cylinder 1, the through channel is connected to a liquid metering delivery pump with a heating device, and the liquid metering delivery pump inlet 5 is connected to the cylinder inner cavity 2.
[0031] Figure 2 The screw assembly diagram in a preferred embodiment of the present invention is shown. As shown in the figure, the twin-screw extruder has a barrel 1, a main feed port 10 located at one end of the barrel, a kneading element 11 for kneading plastic resin and light and heat aging inhibitor, a through channel is opened on the top of the barrel 1 behind the kneading element 11, the through channel is connected to a liquid metering delivery pump with a heating device, the liquid metering delivery pump inlet 5 is connected to the inner cavity of the barrel, and the screw thread elements from the pump inlet to the die head are all conveying elements 7; a vacuum device is provided between the pump inlet and the die head, including a vacuum chamber 8 and a vacuum gauge 9. Figure 2 The numbers below indicate the size of the threaded elements that make up the screw.
[0032] In some embodiments, the through-channel has a diameter of 3-10 mm.
[0033] In some embodiments, the pump inlet is 50-100 cm away from the die.
[0034] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0035] In the present invention, the word "comprise" or its variations, such as "including", "containing", "having" will be understood to include the stated elements, integers or steps, or a combination of elements, integers or steps, but does not exclude the addition of other elements, integers or steps, or a combination of elements, integers or steps.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those of ordinary skill in the art to which the invention belongs. In the event of a conflict, the present specification (including definitions) shall prevail. In addition, the materials, methods and examples are illustrative only and are not intended to be limiting.
[0037] Unless otherwise stated, the numerical ranges listed in the present invention include the endpoint values therein and all point values that increase or decrease in the smallest unit of the endpoint values and all sub-ranges composed of these point values. Unless otherwise stated, the numerical values in the present invention represent the approximate measurement or limitation of the scope of the embodiments including slight deviations from the given values and having approximately the mentioned values and having the mentioned exact values. Except for the last embodiment described in detail, all numerical values of the parameters (e.g., quantity or condition) in the present application document (including the attached claims) should be understood to be modified by the term "approximately" in all cases, regardless of whether "approximately" actually appears before the numerical value. "Approximately" means that the numerical value described allows a slight imprecision (some close to precision in this value; approximately or reasonably close to this value; approximately). If the imprecision provided by "approximately" is not understood in this art with this common meaning, then the "approximately" used herein at least represents the changes that can be produced by the common methods of measuring and using these parameters. For example, “about” can include a variation of less than or equal to 15%, less than or equal to 10%, less than or equal to 5%, less than or equal to 4%, less than or equal to 3%, less than or equal to 2%, less than or equal to 1%, less than or equal to 0.5%, less than or equal to 0.1%, and in some aspects, less than or equal to 0.01%.
[0038] The present invention has been described in detail above, but the present invention is not limited to the above content. In order to keep the description of the embodiments of the present invention clear and concise, the present invention omits the detailed description of known functions and known components.
[0039] Beneficial Effects
[0040] The present invention ultrasonically disperses the luminescent powder in a liquid conveying agent to avoid agglomeration of the luminescent powder, and after being pumped into a twin-screw extruder by a liquid metering delivery pump, the luminescent powder is wrapped by molten plastic, and has a shorter residence time in the twin-screw extruder, and basically does not rub against the metal wall, thereby avoiding the blackening of the metal due to friction.
[0041] In the present invention, all the screw thread elements between the pump inlet and the die head are conveying elements, which can further reduce the situation where the luminescent powder is sheared and blackened by the screw.
[0042] The long-light-storage material prepared by the invention does not turn black, has high luminous intensity and long luminous time, and the luminous time in a dark environment exceeds 12 hours. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a front view, a left view, and a top view of the inlet barrel of the twin-screw extruder connected to the pump in the present invention;
[0044] Figure 2 It is a screw assembly diagram in a preferred embodiment of the present invention.
[0045] Reference numerals:
[0046] 1. Cylinder, 2. Cylinder cavity, 3. Alloy bushing, 4. Positioning pin, 5. Liquid metering pump access port, 6. Cylinder connecting bolt hole, 7. Conveying element, 8. Vacuum chamber, 9. Vacuum gauge, 10. Main feeding port, 11. Kneading element DETAILED DESCRIPTION
[0047] The present invention is further explained below in conjunction with specific examples, which are merely illustrative and exemplary and are not limiting. The equipment, methods and reagents used therein, unless otherwise specified, are all conventional equipment, methods and reagents in the art.
[0048] Reagents and Equipment:
[0049] Phosphorescent powder: JPG-398 purchased from Foshan Juliang Optical Materials Co., Ltd., with a molecular formula of SrAl2O4:Eu~(2+),Dy~(3+), and components by weight percentage of 50-60% strontium carbonate, 35-45% aluminum oxide, 1-3% dysprosium oxide, and 1-2% europium oxide.
[0050] The PE resin was 2720A purchased from Maoming Branch of Sinopec.
[0051] The PP resin was 9025 purchased from Maoming Branch of Sinopec.
[0052] The ABS resin is PA-758 purchased from Chi Mei Company.
[0053] The PA6 resin was M2500I purchased from Chi Mei Company.
[0054] AK-1000 was purchased from Wacker Chemie AG.
[0055] Silane coupling agents KH550, KH560 and KH792 were purchased from Hangzhou Feidian Chemical Co., Ltd.
[0056] Antioxidant 1010 was purchased from BASF.
[0057] Antioxidant 168 was purchased from BASF.
[0058] Antioxidant 1076 was purchased from BASF.
[0059] Antioxidant 1098 was purchased from BASF.
[0060] UV3853PP5 was purchased from Cytec.
[0061] Light stabilizer 770 was purchased from Cytec.
[0062] The light stabilizer UV-P was purchased from Cytec.
[0063] The ultraviolet absorber UV-3808P was purchased from Cytec Corporation.
[0064] Light stabilizer 3346 was purchased from Cytec.
[0065] Light stabilizer 1164 was purchased from Cytec.
[0066] The extrusion equipment adopts Nanjing Ruiya 75 twin-screw extruder, but a through channel with a diameter of 8mm is opened on the top of the barrel, connected to a liquid metering delivery pump with a heating device, the pump inlet is 90cm away from the die head, and the screw thread elements from the pump inlet to the die head are all conveying elements; a vacuum device is set between the pump inlet and the die head, 40cm away from the die head.
[0067] Example 1
[0068] After mixing PE resin and anti-light and heat aging agent for 2 minutes, enter the twin-screw extruder at the main feeding port for kneading and heating and melting. Ultrasonic dispersion of luminescent powder in liquid conveying agent for 4 minutes, then pumped into the twin-screw extruder through the liquid metering pump, mixed with molten plastic and extruded through the die head. Finally, after water cooling and pelletizing, long luminescent material is obtained. The temperature of the liquid metering pump is 30℃, the temperature of the extruder is 160-200℃, and the vacuum degree is -0.08MPa.
[0069] The long light-storage material is composed of the following components in parts by weight: 93.3 parts of PE resin, 0.7 parts of light and heat aging protection agent (1010:168:UV3853PP5:3346=0.1:0.2:0.2:0.2), 3 parts of light-storage powder, and 3 parts of AK-1000 as a liquid delivery agent.
[0070] Example 2
[0071] After mixing PP resin and anti-light and heat aging agent for 3 minutes, enter the twin-screw extruder at the main feeding port for kneading and heating and melting. Ultrasonic dispersion of luminescent powder in liquid conveying agent for 3 minutes, then pumped into the twin-screw extruder through the liquid metering pump, mixed with molten plastic and extruded through the die head. Finally, after water cooling and pelletizing, long luminescent material is obtained. The temperature of the liquid metering pump is 30℃, the temperature of the extruder is 180-220℃, and the vacuum degree is -0.08MPa.
[0072] The long light-storage material is composed of the following components in parts by weight: 93.2 parts of PP resin, 0.8 parts of light and heat aging protection agent (1010:168:3808=0.2:0.2:0.4), 2 parts of light-storage powder, and 4 parts of KH560 as a liquid delivery agent.
[0073] Example 3
[0074] After mixing ABS resin and anti-light and heat aging agent for 2 minutes, enter the twin-screw extruder at the main feeding port for kneading and heating and melting. Ultrasonic dispersion of luminescent powder in liquid conveying agent for 5 minutes, then pumped into the twin-screw extruder through the liquid metering pump, mixed with molten plastic and extruded through the die head. Finally, after water cooling and pelletizing, long luminescent material is obtained. The temperature of the liquid metering pump is 35℃, the temperature of the extruder is 220-240℃, and the vacuum degree is -0.08MPa.
[0075] The long light-storage material is composed of the following components in parts by weight: 91 parts of ABS resin, 1.2 parts of light and heat aging protection agent (1076:168:770:UV-P=0.2:0.2:0.4:0.4), 3.8 parts of light-storage powder, and 4 parts of KH560 as a liquid delivery agent.
[0076] Example 4
[0077] After mixing PA6 resin and anti-light and heat aging agent for 3 minutes, enter the twin-screw extruder at the main feeding port for kneading and heating and melting. Ultrasonic dispersion of luminescent powder in liquid conveying agent for 8 minutes, then pumped into the twin-screw extruder through the liquid metering pump, mixed with molten plastic and extruded through the die head. Finally, after water cooling and pelletizing, long luminescent material is obtained. The temperature of the liquid metering pump is 35℃, the temperature of the extruder is 220-240℃, and the vacuum degree is -0.08MPa.
[0078] The long light-storage material is composed of the following components in parts by weight: 91 parts of PA6 resin, 1 part of light and heat aging protection agent (1098:168:3346:1164=0.2:0.2:0.3:0.3), 4 parts of light-storage powder, and 4 parts of KH550 as a liquid delivery agent.
[0079] Comparative Example 1
[0080] The raw materials and equipment were the same as those in Example 1, except that after all the raw materials were mixed for 2 minutes, they were fed into the twin-screw extruder from the main feeder for extrusion, water cooling, pelletizing, and the liquid metering pump was turned off. The extruder temperature was 160-200°C and the vacuum degree was -0.08MPa.
[0081] Comparative Example 2
[0082] The raw materials and equipment were the same as those in Example 2, except that after all the raw materials were mixed for 3 minutes, they were fed into the twin-screw extruder from the main feeder for extrusion, water cooling, pelletizing, and the liquid metering pump was turned off. The extruder temperature was 180-220° C. and the vacuum degree was -0.08 MPa.
[0083] Comparative Example 3
[0084] The raw materials and equipment were the same as those in Example 3, except that after all the raw materials were mixed for 2 minutes, they were fed into the twin-screw extruder from the main feeder for extrusion, water cooling, pelletizing, and the liquid metering pump was turned off. The extruder temperature was 220-240° C. and the vacuum degree was -0.08 MPa.
[0085] Comparative Example 4
[0086] The raw materials and equipment were the same as those in Example 4, except that after all the raw materials were mixed for 3 minutes, they were fed into the twin-screw extruder from the main feeder for extrusion, water cooling, pelletizing, and the liquid metering pump was turned off. The extruder temperature was 220-240° C. and the vacuum degree was -0.08 MPa.
[0087] The detection method is as follows:
[0088] The long light-storage materials prepared in Examples 1-4 and Comparative Examples 1-4 were injection molded into 60*100 mm flat plates on an injection molding machine. The injection molding temperature of Example 1 and Comparative Example 1 was 160-200°C, the injection molding temperature of Example 2 and Comparative Example 2 was 180-220°C, and the injection molding temperature of Examples 3, 4 and Comparative Examples 3, 4 was 220-240°C.
[0089] Appearance: Visually observe the plate under D65 light source to see if it is black.
[0090] Luminescence brightness: After the D65 light source irradiates the plate for 10 minutes, the luminescence intensity 10 seconds after excitation is recorded by an afterglow intensity tester.
[0091] Luminous time: After the D65 light source irradiates the flat panel for 10 minutes, the luminous intensity drops to 0.32mcd / m -2 time (the lowest brightness visible to the naked eye is 0.32mcd / m -2 ).
[0092] The test results are shown in Table 1:
[0093] Table 1 Appearance effect and brightness test results
[0094] Appearance <![CDATA[Luminous intensity (mcd / m 2 )]]> Luminous time (h) Example 1 No blackening 3338 22 Example 2 No blackening 2485 18 Example 3 No blackening 3316 22 Example 4 No blackening 3772 24 Comparative Example 1 Slightly black, with black threads 1140 9 Comparative Example 2 Slightly black 898 7 Comparative Example 3 Obvious darkening with dark spots 1021 7 Comparative Example 4 Obvious darkening with dark spots 1233 8
[0095] It can be seen from the above table that, by comparing Example 1 and Comparative Example 1, Example 2 and Comparative Example 2, Example 3 and Comparative Example 3, and Example 4 and Comparative Example 4, the twin-screw extrusion equipment of the present invention is used, and the luminescent powder is ultrasonically dispersed in the liquid conveying agent and then pumped into the twin-screw extruder, and a screw composed of a full conveying block threaded element and a vacuum pump are used to prepare long luminescent materials of different resins, which have no blackening phenomenon on the surface, high luminous intensity, and long luminous time, and can meet the requirements of being used in a dark environment for a long time at night.
[0096] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A long light-storage material, prepared from the following components in parts by weight: 74-97.2 parts of plastic resin, 0.5-1 parts of light-heat aging protection agent, 2-20 parts of light-storage powder, and 0.3-5 parts of liquid transport agent.
2. The long-life light-storage material according to claim 1, characterized in that: The plastic resin is selected from: PE, PP, ABS, PA6; and / or The photothermal aging prevention agent includes a heat aging prevention agent and a light aging prevention agent, wherein the heat aging prevention agent is selected from antioxidant 1010, antioxidant 1076, antioxidant 1098, and antioxidant 168; the light aging prevention agent is selected from light stabilizer 770, light stabilizer UV3853PP5, light stabilizer UV-P, ultraviolet absorber UV-3808, light stabilizer 3346, and light stabilizer 1164; and / or The molecular formula of the long-lasting light-storage powder is SrAl2O4:Eu~(2+),Dy~(3+), and the components are 50-60% strontium carbonate, 35-45% aluminum oxide, 1-3% dysprosium oxide, and 1-2% europium oxide by weight; and / or The liquid delivery agent is selected from diffusion oil Wacker Ak-1000, silane coupling agent KH550, KH560, KH792.
3. The long-life light-storage material according to claim 1, characterized in that: The plastic resin is PE, the liquid delivery agent is selected from diffusion oil Wacker Ak-1000, silane coupling agent KH550, KH560, KH570, KH792, and the light and heat aging protection agent is 1010:168:UV3853PP5:3346=0.1-0.3:0.1-0.3:0.2-0.4:02-0.4; or The plastic resin is PP, the liquid delivery agent is selected from diffusion oil Wacker Ak-1000, silane coupling agent KH550, KH560, KH792, and the light and heat aging protection agent is 1010:168:3808=0.1-0.4:0.1-0.4:0.2-0.8; or The plastic resin is ABS, the liquid delivery agent is selected from diffusion oil Wacker Ak-1000, silane coupling agent KH550, KH560, KH792, and the light and heat aging protection agent is 1076:168:770:UV-P=0.1-0.3:0.1-0.3:0.2-0.4:02-0.4; or The plastic resin is PA6, the liquid delivery agent is selected from diffusion oil Wacker Ak-1000, one of silane coupling agents KH550, KH560, and KH792, and the light and heat aging protection agent is 1098:168:3346:1164=0.1-0.3:0.1-0.3:0.2-0.4:02-0.
4.
4. The long-life light-storage material according to any one of claims 1 to 3, characterized in that: The long light storage material is prepared by the following method, which is carried out in a twin-screw extruder, wherein a through channel is opened at the top of the barrel of the twin-screw, the through channel is connected to a liquid metering delivery pump with a heating device, the distance between the pump inlet and the die head is 20-100 cm, and the screw thread elements from the pump inlet to the die head are all delivery elements; a vacuum device is provided between the pump inlet and the die head, and the distance from the die head is 40-50 cm, and the method comprises the following steps: Plastic resin and anti-light and heat aging agent are added from the main feeding port and heated and melted by a twin-screw extruder; the luminescent powder is first dispersed in a liquid conveying agent by ultrasonic wave, and then pumped into the extruder barrel through the top of the barrel by a liquid metering delivery pump to mix with the molten plastic and extrude through a die head, cool, and pelletize.
5. The long-life light-storage material according to claim 4, characterized in that: The ultrasonic dispersion time is 0.2-10 min; and / or The temperature of the liquid metering delivery pump is set to 20-60° C.; and / or The diameter of the through channel is 3-10 mm; and / or The distance between the pump inlet and the die head is 50-100 cm.
6. The long-life light-storage material according to claim 4, characterized in that: The plastic resin is PE, the extrusion temperature is 160-200°C, and the vacuum degree is ≤-0.08MPa; or The plastic resin is PP, the extrusion temperature is 180-220°C, and the vacuum degree is ≤-0.08MPa; or The plastic resin is ABS, the extrusion temperature is 220-240°C, and the vacuum degree is ≤-0.08MPa; or The plastic resin is PA6, the extrusion temperature is 220-240° C., and the vacuum degree is ≤-0.08 MPa.
7. A method for preparing the long light-storage material according to any one of claims 1 to 3, wherein the method is carried out in a twin-screw extruder, a through channel is provided at the top of the barrel of the twin-screw, the through channel is connected to a liquid metering delivery pump with a heating device, the distance between the pump inlet and the die head is 20-100 cm, and all the screw thread elements from the pump inlet to the die head are delivery elements; a vacuum device is provided between the pump inlet and the die head, and the distance from the die head to the vacuum device is 40-50 cm. The method comprises the following steps: Plastic resin and anti-light and heat aging agent are added from the main feeding port and heated and melted by a twin-screw extruder; the luminescent powder is first dispersed in a liquid conveying agent by ultrasonic wave, and then pumped into the extruder barrel through the top of the barrel by a liquid metering delivery pump to mix with the molten plastic and extrude through a die head, cool, and pelletize.
8. The method according to claim 7, characterized in that The ultrasonic dispersion time is 0.2-10 min; and / or The temperature of the liquid metering delivery pump is set to 20-60° C.; and / or The diameter of the through channel is 3-10 mm; and / or The distance between the pump inlet and the die head is 50-100 cm.
9. The method according to claim 7, characterized in that: The plastic resin is PE, the extrusion temperature is 160-200°C, and the vacuum degree is ≤-0.08MPa; or The plastic resin is PP, the extrusion temperature is 180-220°C, and the vacuum degree is ≤-0.08MPa; or The plastic resin is ABS, the extrusion temperature is 220-240°C, and the vacuum degree is ≤-0.08MPa; or The plastic resin is PA6, the extrusion temperature is 220-240° C., and the vacuum degree is ≤-0.08 MPa.
10. An extrusion device for preparing a long-lasting light-storage material, the extrusion device being a twin-screw extruder, characterized in that: A through channel is opened on the top of the barrel, and the through channel is connected to a liquid metering delivery pump with a heating device. The distance between the pump inlet and the die head is 20-100 cm, and all the screw thread elements from the pump inlet to the die head are delivery elements; a vacuum device is provided between the pump inlet and the die head, and the distance from the die head is 40-50 cm; Particularly, the diameter of the through-channel is 3-10 mm; and / or the distance between the pump inlet and the die head is 50-100 cm.
Citation Information
Patent Citations
Long-acting luminous engineering plastic and preparation method thereof
CN102585471A
Luminous plastic, double-screw extruding machine for preparing luminous plastic and preparation method
CN107815018A
TPU noctilucent master batch and preparation method thereof
CN110982249A
Noctilucent suede material as well as preparation method and application thereof
CN115094635A
Production of thermoplastic resin composition containing luminous fluorescent substance