Anti-corrosion PE pipe and production process thereof

By using a combination of modified high-density polyethylene and other additives in PE pipes, the problem of poor corrosion resistance in high-temperature environments is solved, and the corrosion resistance and UV aging resistance are significantly improved, ensuring the long-term use of the pipes stability.

CN118956089APending Publication Date: 2024-11-15NANYANG SENYUAN PLASTIC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411176733.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Traditional PE pipes have poor corrosion resistance in high-temperature corrosion environments, which affects service life and safety performance.

Method used

Modified high-density polyethylene is used as the matrix resin, and polyimide, polyether ether ketone, polytetrafluoroethylene, silane coupling agent modified filler and antioxidant are added to improve corrosion resistance through grafting and uniform dispersion.

Benefits of technology

It significantly improves the corrosion resistance of PE pipes in high-temperature corrosion environments, and enhances the resistance to ultraviolet aging, ensuring the long-term stability of the pipes in normal temperature and high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010918480000061
    Figure BDA0005010918480000061
  • Figure BDA0005010918480000071
    Figure BDA0005010918480000071
  • Figure BDA0005010918480000072
    Figure BDA0005010918480000072
Patent Text Reader

Abstract

The invention discloses an anti-corrosion PE pipe and a production process thereof, and relates to the field of pipes. The anti-corrosion pipe is prepared from, by weight, 100 parts of modified high-density polyethylene, 2-3 parts of polyimide, 2-4 parts of polyether-ether-ketone, 1.5-2.5 parts of polytetrafluoroethylene, 2-4 parts of silane coupling agent modified filler and 1-2 parts of antioxidant, and the modified high-density polyethylene is prepared from maleic anhydride, 1, 2-propylene glycol and 1, 3-propylene glycol. The invention discloses a high-density polyethylene composite material which comprises maleic anhydride, 1, 2-epoxy-5-hexene, vinyl silicone oil, high-density polyethylene and an initiator, and the weight ratio of the maleic anhydride to the 1, 2-epoxy-5-hexene to the vinyl silicone oil to the high-density polyethylene to the initiator is (5.4-7.8): (4.2-6.5): (7.2-9.4): 100: (1-2). The anti-corrosion PE pipe has excellent acid, alkali and salt corrosion resistance no matter in a normal-temperature corrosion environment or a high-temperature corrosion environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of pipes, and in particular to an anti-corrosion PE pipe and a production process thereof. Background Art

[0002] Polyethylene (PE) pipes are widely used in urban and rural water supply, gas transmission, sewage treatment and agricultural irrigation due to their lightness, durability and easy installation. However, traditional PE pipes are prone to corrosion and aging after long-term use, especially in corrosive environments, which affects their service life and safety performance. Therefore, improving the corrosion resistance of PE pipes has become an urgent problem to be solved in the industry.

[0003] At present, in order to improve the corrosion resistance of PE pipes, high-density polyethylene is usually used as the base resin of anti-corrosion PE pipes in related technologies. Among them, high-density polyethylene has excellent corrosion resistance in normal temperature corrosion environment. However, in the face of some harsh environments, such as high temperature corrosion environment, the corrosion resistance of high-density polyethylene is poor. Summary of the invention

[0004] In order to improve the anti-corrosion performance of the anti-corrosion pipe in the related art in a high-temperature corrosive environment, the present application provides an anti-corrosion PE pipe and a production process thereof.

[0005] In the first aspect, the present application provides an anti-corrosion PE pipe adopting the following technical solution: A corrosion-resistant pipe comprises 100 parts by weight of modified high-density polyethylene, 2-3 parts by weight of polyimide, 2-4 parts by weight of polyetheretherketone, 1.5-2.5 parts by weight of polytetrafluoroethylene, 2-4 parts by weight of silane coupling agent modified filler and 1-2 parts by weight of antioxidant. The raw materials of the modified high-density polyethylene comprise maleic anhydride, 1,2-epoxy-5-hexene, vinyl silicone oil, high-density polyethylene and an initiator. The weight ratio of the maleic anhydride, 1,2-epoxy-5-hexene, vinyl silicone oil, high-density polyethylene and initiator is (5.4-7.8):(4.2-6.5):(7.2-9.4):100:(1-2).

[0006] In the present application, the anti-corrosion pipe adopts the modified high-density polyethylene obtained by grafting maleic anhydride, 1,2-epoxy-5-hexene and vinyl silicone oil on high-density polyethylene as the base resin, wherein, compared with the high-density polyethylene before modification, the modified high-density polyethylene after grafting modification has better high-temperature resistance and corrosion resistance. At the same time, the present application also adds polyimide, polyetheretherketone, polytetrafluoroethylene and silane coupling agent modified fillers. Since polyimide, polyetheretherketone, polytetrafluoroethylene and silane coupling agent modified fillers have good compatibility with modified high-density polyethylene, the anti-corrosion performance of the anti-corrosion pipe in a high-temperature corrosion environment can be improved by the combination of polyimide, polyetheretherketone, polytetrafluoroethylene and silane coupling agent modified fillers with modified high-density polyethylene. In addition, the addition of antioxidants can prevent the degradation of polymers during processing, and is also beneficial to the corrosion resistance of anti-corrosion pipes in a high-temperature corrosion environment.

[0007] In some specific embodiments, the density of the high-density polyethylene is 0.94-0.97 g / cm 3 , the melt index is 7-8g / 10min (190℃ / 2.16kg).

[0008] In this application, the preferred density of high-density polyethylene is 0.94-0.97 g / cm 3 , high-density polyethylene with a melt index of 7-8g / 10min (190℃ / 2.16kg) has good anti-corrosion properties and is also conducive to uniform dispersion of various raw materials.

[0009] In some specific embodiments, the structural formula of the vinyl silicone oil is: CH2=CHSi(R)2O[Si(R)2O] n (R)2SiCH=CH2, wherein R is at least one of an alkyl group and a phenyl group.

[0010] Compared with the use of single vinyl-terminated silicone oil, the vinyl silicone oil in this application is preferably double vinyl-terminated silicone oil, which is beneficial to further improve the high temperature and corrosion resistance of the anti-corrosion pipe, and can also improve the ultraviolet aging resistance of the anti-corrosion PE pipe.

[0011] In some specific embodiments, R is more preferably phenyl.

[0012] In the present application, R in the vinyl silicone oil is preferably phenyl, that is, the vinyl silicone oil is further preferably divinyl-terminated phenyl silicone oil, which is beneficial to further improve the UV aging resistance of the anti-corrosion PE pipe.

[0013] In some specific implementations, the value of n is 10-15.

[0014] In the present application, the value of n in the vinyl silicone oil is preferably 10-15, which is beneficial to improving the grafting rate of the vinyl silicone oil and obtaining a PE pipe with good high temperature resistance, corrosion resistance and UV aging resistance.

[0015] In some specific embodiments, the particle size of the polytetrafluoroethylene is in the range of 1-10 μm.

[0016] In the present application, the particle size range of polytetrafluoroethylene is preferably 1-10 μm, which is conducive to the uniform dispersion of polytetrafluoroethylene in the modified high-density polyethylene.

[0017] In some specific embodiments, the silane coupling agent modified filler is at least one of an isocyanate silane coupling agent modified filler and an epoxy silane coupling agent modified filler.

[0018] In the present application, the silane coupling agent modified filler adopts at least one of an isocyanate silane coupling agent modified filler or an epoxy silane coupling agent modified filler, which is beneficial to improve the dispersibility of the filler in the modified high-density polyethylene.

[0019] In some specific embodiments, the antioxidant includes antioxidant 1010 and antioxidant 168, and the weight ratio of antioxidant 1010 to antioxidant 168 is (3-4):1.

[0020] In the present application, the antioxidant adopts a composition of antioxidant 1010 and antioxidant 168 in a weight ratio of (3-4):1, which is beneficial to improve the high temperature corrosion resistance and ultraviolet aging resistance of the anti-corrosion PE pipe.

[0021] In some specific embodiments, the anti-corrosion pipe further comprises 2.5-3.5 parts by weight of masterbatch.

[0022] In the actual production process, color masterbatch can also be added according to actual needs to obtain anti-corrosion pipes of the desired color.

[0023] In the second aspect, the production process of a corrosion-resistant PE pipe provided in the present application adopts the following technical solution: A production process for anti-corrosion PE pipes comprises the following steps: After high-density polyethylene is melted, maleic anhydride, 1,2-epoxy-5-hexene, vinyl silicone oil and initiator are added, the temperature is raised to 175-185°C, kneading reaction is carried out for 2-3 hours, followed by extrusion and granulation to obtain modified high-density polyethylene; After the modified high-density polyethylene is fully melted at 200-210°C, polyimide, polyetheretherketone, polytetrafluoroethylene, silane coupling agent modified filler and antioxidant are added in sequence, and the melting is continued to be uniform, followed by extrusion and cooling to obtain an anti-corrosion PE pipe.

[0024] The present application first adopts maleic anhydride, 1,2-epoxy-5-hexene and vinyl silicone oil to graft-modify high-density polyethylene to obtain modified high-density polyethylene, then fully melts the modified high-density polyethylene, and then successively adds polyimide, polyetheretherketone, polytetrafluoroethylene and other raw materials, and finally extrude and cool to form an anti-corrosion PE pipe. The pipe has excellent anti-corrosion performance whether in a normal temperature corrosion environment or a high temperature corrosion environment.

[0025] In summary, this application at least includes the following beneficial technical effects: (1) The anti-corrosion pipe in the present application adopts the modified high-density polyethylene obtained by grafting high-density polyethylene with maleic anhydride, 1,2-epoxy-5-hexene and vinyl silicone oil as the base resin, wherein the modified high-density polyethylene after grafting has better high-temperature resistance and corrosion resistance than the high-density polyethylene before modification. At the same time, the present application also adds polyimide, polyetheretherketone, polytetrafluoroethylene and silane coupling agent modified fillers. Since polyimide, polyetheretherketone, polytetrafluoroethylene and silane coupling agent modified fillers have good compatibility with modified high-density polyethylene, the anti-corrosion performance of the anti-corrosion pipe in a high-temperature corrosion environment can be improved by combining polyimide, polyetheretherketone, polytetrafluoroethylene and silane coupling agent modified fillers with modified high-density polyethylene. In addition, the addition of antioxidants can prevent the degradation of polymers during processing, which is also beneficial to the corrosion resistance of the anti-corrosion pipe in a high-temperature corrosion environment.

[0026] (2) Compared with the use of monovinyl-terminated silicone oil, the vinyl silicone oil in the present application is preferably divinyl-terminated silicone oil, which is beneficial to further improve the high temperature and corrosion resistance of the anti-corrosion pipe, and can also improve the UV aging resistance of the anti-corrosion PE pipe. DETAILED DESCRIPTION

[0027] The present application is further described below in conjunction with specific experiments. Example

[0028] [Example 1] A corrosion-resistant PE pipe comprises 100 kg of modified high-density polyethylene, 2 kg of polyimide (Mitsui, Japan, TPIJ3124), 4 kg of polyetheretherketone (Solvay, USA, KT-880GF15), 1.5 kg of polytetrafluoroethylene (DuPont, USA, TE3859), 4 kg of silane coupling agent modified filler (obtained by uniformly mixing 3-isocyanatepropyltrimethoxysilane and nano calcium carbonate in a weight ratio of 1:8), 0.75 kg of antioxidant 1010 and 0.25 kg of antioxidant 168.

[0029] Among them, the modified high-density polyethylene includes 5.4kg of maleic anhydride, 6.5kg of 1,2-epoxy-5-hexene, 7.2kg of vinyl silicone oil (specifically, terminal vinyl and terminal hydroxyl polydimethylsiloxane, the degree of polymerization of the dimethylsiloxane segment is 10), 100kg of high-density polyethylene (Lotte Chemical, 2700J, the melt index at 190℃ / 2.16kg is 7g / 10min) and 1kg of initiator (specifically, benzoyl peroxide).

[0030] In this embodiment, the production process of the anti-corrosion PE pipe includes the following steps: After high-density polyethylene is melted, maleic anhydride, 1,2-epoxy-5-hexene, vinyl silicone oil and initiator are added, the temperature is raised to 175°C, kneading reaction is carried out for 3 hours, and then extrusion and pelletization are carried out to obtain modified high-density polyethylene; After the modified high-density polyethylene is fully melted at 200°C, polyimide, polyetheretherketone, polytetrafluoroethylene, silane coupling agent modified filler, antioxidant 1010 and antioxidant 168 are added in sequence, and the melting is continued to be uniform, followed by extrusion and cooling to obtain a corrosion-resistant PE pipe.

[0031] [Example 2] A corrosion-resistant PE pipe comprises 100 kg of modified high-density polyethylene, 3 kg of polyimide (Mitsui, TPIJ3124), 2 kg of polyetheretherketone (Degussa, 2000CF30), 2.5 kg of polytetrafluoroethylene (Daikin, F-L2), 2 kg of silane coupling agent modified filler (obtained by uniformly mixing γ-glycidyloxypropyltrimethoxysilane and nano calcium carbonate in a weight ratio of 1:10), 1.6 kg of antioxidant 1010 and 0.4 kg of antioxidant 168.

[0032] Among them, the modified high-density polyethylene includes 7.8kg of maleic anhydride, 4.2kg of 1,2-epoxy-5-hexene, 9.4kg of vinyl silicone oil (specifically, terminal vinyl and terminal hydroxyl polydimethylsiloxane, the degree of polymerization of the dimethylsiloxane segment is 10), 100kg of high-density polyethylene (ExxonMobil, HMA-025, the melt index at 190℃ / 2.16kg is 8g / 10min) and 2kg of initiator (specifically, diisopropyl peroxide).

[0033] In this embodiment, the production process of the anti-corrosion PE pipe includes the following steps: After high-density polyethylene is melted, maleic anhydride, 1,2-epoxy-5-hexene, vinyl silicone oil and initiator are added, the temperature is raised to 185°C, kneading reaction is carried out for 2 hours, and then extrusion and pelletization are carried out to obtain modified high-density polyethylene; After the modified high-density polyethylene is fully melted at 210°C, polyimide, polyetheretherketone, polytetrafluoroethylene, silane coupling agent modified filler, antioxidant 1010 and antioxidant 168 are added in sequence, and the melting is continued to be uniform, followed by extrusion and cooling to obtain a corrosion-resistant PE pipe.

[0034] [Example 3] A corrosion-resistant PE pipe, which differs from [Example 1] in that the type of vinyl silicone oil used in the modified high-density polyethylene is different.

[0035] The vinyl silicone oil in this embodiment is specifically divinyl-terminated methyl silicone oil, and the structural formula of divinyl-terminated methyl silicone oil is CH2=CHSi(CH3)2O[Si(CH3)2O] 10 (CH3)2SiCH=CH2.

[0036] [Example 4] A corrosion-resistant PE pipe, which differs from [Example 1] in that the type of vinyl silicone oil used in the modified high-density polyethylene is different.

[0037] The vinyl silicone oil in this embodiment is specifically divinyl-terminated phenyl silicone oil, and the structural formula of divinyl-terminated phenyl silicone oil is CH2=CHSi(C6H5)2O[Si(C6H5)2O] 10 (C6H5)2SiCH=CH2.

[0038] [Example 5] A corrosion-resistant PE pipe, which differs from [Example 4] in that: in the divinyl-terminated phenyl silicone oil, the value of the polymerization degree n of the phenylsiloxane chain segment is different. In this example, the value of n is 15.

[0039] [Example 6] A corrosion-resistant PE pipe, which differs from [Example 1] in that: in the divinyl-terminated phenyl silicone oil, the value of the polymerization degree n of the phenylsiloxane chain segment is different. In this embodiment, the value of n is 25.

[0040] Comparative Example [Comparative Example 1] A corrosion-resistant PE pipe, which differs from [Example 1] in that maleic anhydride is not added when preparing the modified high-density polyethylene.

[0041] [Comparative Example 2] A corrosion-resistant PE pipe, which differs from [Example 1] in that: when preparing modified high-density polyethylene, 1,2-epoxy-5-hexene is replaced by an equal amount of vinyl silicone oil (specifically, vinyl-terminated hydroxyl-terminated polydimethylsiloxane, the degree of polymerization of the dimethylsiloxane chain segment is 10).

[0042] [Comparative Example 3] A corrosion-resistant PE pipe, which differs from [Example 1] in that when preparing modified high-density polyethylene, the vinyl silicone oil is replaced by an equal amount of 1,2-epoxy-5-hexene.

[0043] [Comparative Example 4] A corrosion-resistant PE pipe, which differs from [Example 1] in that polyimide is replaced by an equal amount of high-density polyethylene (Lotte Chemical, 2700J, melt index of 7g / 10min at 190°C / 2.16kg).

[0044] [Comparative Example 5] A corrosion-resistant PE pipe, which differs from [Example 1] in that polyetheretherketone is replaced by an equal amount of high-density polyethylene (Lotte Chemical, 2700J, melt index of 7g / 10min at 190°C / 2.16kg).

[0045] [Comparative Example 6] A corrosion-resistant PE pipe, which differs from [Example 1] in that polytetrafluoroethylene is replaced by an equal amount of high-density polyethylene (Lotte Chemical, 2700J, melt index of 7g / 10min at 190°C / 2.16kg).

[0046] Performance testing 1. Test 1. According to GB / T 6111-2018 Determination of the internal pressure resistance of thermoplastic pipe systems for fluid transportation, the test was conducted, and the examples and comparative examples were recorded to determine whether rupture, leakage, etc. occurred within the specified test pressure and test time. The test medium was water, the test temperature was 20°C, the test pressure was 12.5MPa or 15MPa, and the specified test time was 100h. Ten PE pipes were randomly selected from each example and comparative example. If the pipe was damaged or leaked within the specified test time, the test was stopped, and the test pressure was reduced by 0.5MPa, and the test was repeated until the tested pipe did not rupture or leak within the specified time, and the maximum test pressure that the pipe could withstand was recorded. Among them, no leakage was qualified when the test pressure was 12.5MPa.

[0047] 2. Test 2: The PE pipes in the embodiments and comparative examples were immersed in 10% sulfuric acid solution, 10% sodium hydroxide solution and 10% sodium chloride solution, respectively, and then the sulfuric acid solution, sodium hydroxide solution and sodium chloride solution were heated to 80°C and immersed at constant temperature for 7 days, and then the immersed PE pipes were washed and dried, and finally the PE pipes were tested again in Test 1. Among them, no leakage was qualified when the test pressure was 12.5MPa.

[0048] 3. Test 3: The PE pipes in each embodiment and comparative example were placed in a hernia lamp aging box for 10,000 hours, and then the PE pipes were tested again in Test 1. When the test pressure was 12.5 MPa, no leakage was considered acceptable.

[0049] Table 1 Internal pressure resistance test before immersion Sample 12.5MPa 15MPa Example 1 No leakage No leakage Example 2 No leakage No leakage Example 3 No leakage No leakage Example 4 No leakage No leakage Example 5 No leakage No leakage Example 6 No leakage No leakage Comparative Example 1 No leakage 2 leaks Comparative Example 2 No leakage No leakage Comparative Example 3 No leakage No leakage Comparative Example 4 No leakage No leakage Comparative Example 5 No leakage No leakage Comparative Example 6 No leakage No leakage Table 2 Internal pressure resistance test after immersion in sulfuric acid Table 3 Internal pressure resistance test after soaking in sodium hydroxide Sample 12.5MPa 15MPa Example 1 No leakage 10 Leaks Example 2 No leakage 10 Leaks Example 3 No leakage 4 Leaks Example 4 No leakage No leakage Example 5 No leakage No leakage Example 6 No leakage 4 Leaks Comparative Example 1 7 Leaks 10 Leaks Comparative Example 2 3 Leaks 10 Leaks Comparative Example 3 8 Leaks 10 Leaks Comparative Example 4 5 Leaks 10 Leaks Comparative Example 5 2 leaks 10 Leaks Comparative Example 6 3 Leaks 10 Leaks Table 4 Internal pressure resistance test after soaking in sodium chloride Table 5 Internal pressure resistance test after aging Sample 12.5MPa 15MPa Example 1 No leakage 10 Leaks Example 2 No leakage 10 Leaks Example 3 No leakage 2 leaks Example 4 No leakage No leakage Example 5 No leakage No leakage Example 6 No leakage 2 leaks Comparative Example 1 3 Leaks 10 Leaks Comparative Example 2 1 Leak 5 Leaks Comparative Example 3 4 Leaks 10 Leaks Comparative Example 4 3 leaks 10 Leaks Comparative Example 5 1 Leak 10 Leaks Comparative Example 6 2 leaks 10 Leaks Combining Example 1 with Comparative Examples 1-6 and the experimental results in Tables 1-5, it can be seen that the grafting raw materials of the modified high-density polyethylene lack any one of maleic anhydride, 1,2-epoxy-5-hexene, and vinyl silicone oil, which is not conducive to obtaining PE pipes with good high-temperature acid, alkali, and salt corrosion resistance. In addition, the aging resistance of the PE pipe is reduced.

[0050] Combining Example 1 with Examples 3-4 and the experimental results in Tables 1-5, it can be seen that compared with the use of monovinyl-terminated silicone oil, the vinyl silicone oil in this application is preferably divinyl-terminated silicone oil, which is beneficial to further improve the high temperature and corrosion resistance of the anti-corrosion pipe, and can also improve the ultraviolet aging resistance of the anti-corrosion PE pipe.

[0051] Combining Examples 4-6 and the experimental results in Tables 1-5, it can be seen that the value of n in the divinyl-terminated phenyl silicone oil is preferably 10-15, which is conducive to obtaining PE pipes with good high-temperature acid, alkali, and salt corrosion resistance and good UV aging resistance.

[0052] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An anti-corrosion PE pipe, characterized by: The invention comprises 100 parts by weight of modified high-density polyethylene, 2-3 parts by weight of polyimide, 2-4 parts by weight of polyetheretherketone, 1.5-2.5 parts by weight of polytetrafluoroethylene, 2-4 parts by weight of silane coupling agent modified filler and 1-2 parts by weight of antioxidant. The raw materials of the modified high-density polyethylene comprise maleic anhydride, 1,2-epoxy-5-hexene, vinyl silicone oil, high-density polyethylene and initiator. The weight ratio of maleic anhydride, 1,2-epoxy-5-hexene, vinyl silicone oil, high-density polyethylene and initiator is (5.4-7.8):(4.2-6.5):(7.2-9.4):100:(1-2).

2. The anti-corrosion PE pipe according to claim 1, characterized in that: The density of the high-density polyethylene is 0.94-0.97 g / cm 3 , the melt index is 7-8g / 10min (190℃ / 2.16kg).

3. The anti-corrosion PE pipe according to claim 1, characterized in that: The structural formula of the vinyl silicone oil is: CH2=CHSi(R)2O[Si(R)2O] n (R)2SiCH=CH2, wherein R is at least one of an alkyl group and a phenyl group.

4. The anti-corrosion PE pipe according to claim 3, characterized in that: R is phenyl.

5. The anti-corrosion PE pipe according to claim 3, characterized in that: The value range of n is 10-15.

6. The anti-corrosion PE pipe according to claim 1, characterized in that: The particle size of the polytetrafluoroethylene is in the range of 1-10 μm.

7. The anti-corrosion PE pipe according to claim 1, characterized in that: The silane coupling agent modified filler is at least one of an isocyanate silane coupling agent modified filler and an epoxy silane coupling agent modified filler.

8. The anti-corrosion PE pipe according to claim 1, characterized in that: The antioxidant includes antioxidant 1010 and antioxidant 168, and the weight ratio of antioxidant 1010 to antioxidant 168 is (3-4):

1.

9. The anti-corrosion PE pipe according to any one of claims 1 to 8, characterized in that: The anti-corrosion pipe also includes 2.5-3.5 parts by weight of masterbatch.

10. A production process for an anti-corrosion PE pipe according to any one of claims 1 to 9, characterized in that: The following steps are involved: After high-density polyethylene is melted, maleic anhydride, 1,2-epoxy-5-hexene, vinyl silicone oil and initiator are added, the temperature is raised to 175-185°C, kneading reaction is carried out for 2-3 hours, followed by extrusion and granulation to obtain modified high-density polyethylene; After the modified high-density polyethylene is fully melted at 200-210°C, polyimide, polyetheretherketone, polytetrafluoroethylene, silane coupling agent modified filler and antioxidant are added in sequence, and the melting is continued to be uniform, followed by extrusion and cooling to obtain an anti-corrosion PE pipe.

Citation Information

Cited By

  • Graft modified polyethylene as well as preparation method and application thereof

    CN121717958A