Polyester core material and preparation method thereof, wind power blade skin and wind power blade

By introducing bisphenol A diglycidyl ethers and methyltetrahydrophthalic acid of wind-powered blade pultrusion plate degradation products into PET materials, the modified polyester is formed, which solves the insufficient heat resistance and mechanical properties of PET resin. The problem is to improve the heat resistance and mechanical strength of the material.

CN118956115AActive Publication Date: 2024-11-15SINOMATECH WIND POWER BLADE

Patent Information

Application Number
CN202411303423.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-15
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

The heat resistance and mechanical properties of existing polyethylene terephthalate (PET) resins are not ideal, and it is difficult to improve their tensile strength and yield strength at the same time.

Method used

By introducing bisphenol A diglycidyl ethers and methyltetrahydrophthalic acid in the degradation product of the wind power blade pultrusion plate, the modified polyester is formed through polycondensation reaction of hydroxyl and carboxyl groups, and the molar ratio of the chain segment is controlled. and molecular weight distribution to improve the heat resistance and mechanical properties of PET materials.

Benefits of technology

The heat resistance and mechanical properties of PET materials have been significantly improved, including improving melt viscosity, thermal deformation temperature, ultimate tensile strength and yield strength, while enhancing the water resistance of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005049532320000011
    Figure BDA0005049532320000011
  • Figure BDA0005049532320000021
    Figure BDA0005049532320000021
  • Figure BDA0005049532320000051
    Figure BDA0005049532320000051
Patent Text Reader

Abstract

The invention provides a polyester core material and a preparation method thereof, a wind power blade skin and a wind power blade, the polyester core material comprises modified polyester, the modified polyester material introduces a chain segment of bisphenol A diglycidyl ether and a chain segment of methyl tetrahydrophthalic acid into a PET material, and the molar ratio of the chain segment of the bisphenol A diglycidyl ether to the chain segment of the ethylene glycol is controlled to be 1: (10-50), so that high-content groups with rigid structures and larger spatial internal resistance can be introduced into the PET material, the number-average molecular weight and the molecular weight of the PET material are distributed in a proper range, the modified polyester molecules are difficult to move, and the PET material has excellent mechanical properties. The heat resistance and the mechanical property of PET are improved at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of polyester materials, and specifically relates to a polyester core material and a preparation method thereof, a wind turbine blade skin and a wind turbine blade. Background Art

[0002] Polyethylene terephthalate (PET in English and polyester in Chinese) core material is mainly obtained by mixing polyethylene terephthalate resin with a foaming agent and foaming. The performance of polyethylene terephthalate core material mainly depends on the properties of the PET resin used. PET resin is low in price, has low abrasion and high hardness, is non-toxic, has good weather resistance and chemical resistance, has low water absorption, and is resistant to weak acids and organic solvents. It is one of the most cost-effective plastic resins, so it is widely used.

[0003] However, the heat resistance and mechanical properties of PET resin are not ideal, and it is especially difficult to obtain PET resin with good heat resistance and mechanical properties. Although there are methods to modify PET resin by increasing the molecular weight of PET or introducing functional additives, these methods still cannot give good consideration to the improvement of heat resistance and mechanical properties, such as tensile strength and yield strength, at the same time. Summary of the invention

[0004] The present application provides a polyester core material and a preparation method thereof, a wind turbine blade skin and a wind turbine blade, aiming to simultaneously improve the heat resistance and mechanical properties of the polyester core material.

[0005] In a first aspect, the present application provides a polyester core material, comprising a modified polyester, wherein the modified polyester comprises segments shown in the following formulas 1, 2, 3 and 4:

[0006]

[0007]

[0008] The chain segment of formula 1 is connected to the chain segment of formula 3 or formula 4; the chain segment of formula 4 is connected to the chain segment of formula 1 or formula 2; the molar ratio of the chain segments of formula 1 to formula 2 is 1:(10-50).

[0009] In a feasible embodiment of the first aspect of the present application, the modified polyester satisfies at least one of the following conditions:

[0011] a. The molar ratio of the chain segments represented by formula 4 to formula 3 is 1:(10-50);

[0012] b. The ratio of the total molar amount of the segments represented by Formula 1 and Formula 2 to the total molar amount of the segments represented by Formula 3 and Formula 4 is 1:(0.6-2), and may be 1:(1.0-1.5);

[0013] c. The weight of the chain segments represented by Formula 1 and Formula 4 accounts for 1% to 20% of the total weight of the modified polyester.

[0014] In a feasible embodiment of the first aspect of the present application, the modified polyester satisfies at least one of the following conditions:

[0015] d. The number average molecular weight of the modified polyester is 20000Da to 30000Da;

[0016] e. The molecular weight distribution of the modified polyester is 1.5 to 2.2;

[0017] f. The hydroxyl value of the modified polyester is 50 mgKOH / g to 150 mgKOH / g.

[0018] In a feasible implementation manner of the first aspect of the present application, the melt viscosity of the modified polyester is 250 Pa·s to 520 Pa·s; and / or the heat deformation temperature of the modified polyester is 100°C to 120°C.

[0019] In a feasible implementation manner of the first aspect of the present application, the ultimate tensile strength of the modified polyester is 40 MPa to 55 MPa; and / or, the yield strength of the modified polyester is 35 MPa to 50 MPa.

[0020] In a feasible implementation of the first aspect of the present application, the polyester core material also includes a foaming agent, and the mass ratio of the modified polyester to the foaming agent is 1:(0.2-0.8); optionally, the foaming agent includes one or more of azodicarbonamide, azobisisobutyronitrile and azodiacetate.

[0021] The second aspect of the present application provides a method for preparing the polyester core material provided in the first aspect of the present application, comprising:

[0022] Providing a degradation product of a wind turbine blade pultruded plate, wherein the degradation product of the wind turbine blade pultruded plate includes components of the chain segments shown in Formula 1 and Formula 4;

[0023] The degradation product of the wind turbine blade pultruded sheet is mixed with terephthalic acid and ethylene glycol to obtain a modified polyester;

[0024] The modified polyester and the foaming agent are mixed and expanded to obtain a polyester core material.

[0025] In a feasible implementation of the second aspect of the present application, in the step of providing a degradation product of a wind turbine blade pultruded plate, wherein the degradation product of the wind turbine blade pultruded plate includes components of the chain segments shown in Formula 1 and Formula 4, the hydroxyl value of the degradation product of the wind turbine blade pultruded plate is 300 mg KOH / g to 400 mg KOH / g.

[0026] In a feasible implementation manner of the second aspect of the present application, in the step of mixing the degradation product of the wind turbine blade pultruded sheet with terephthalic acid and ethylene glycol to obtain the modified polyester, the degradation product of the wind turbine blade pultruded sheet is reacted with terephthalic acid and ethylene glycol in an inert atmosphere and a vacuum degree of 0Pa to 10Pa at 240°C to 300°C for 5h to 12h to obtain the modified polyester.

[0027] In a feasible implementation manner of the second aspect of the present application, in the step of mixing the modified polyester and the foaming agent and expanding them to obtain the polyester core material, the modified polyester and the foaming agent are mixed and stirred in a mass ratio of 1:(0.2~0.8), stirred for 2h~10h in a nitrogen atmosphere at 240℃~260℃, and cooled to room temperature to fix, so as to obtain the PET core material.

[0028] The third aspect of the present application provides a wind turbine blade skin, comprising the polyester core material provided in the first aspect of the present application.

[0029] A fourth aspect of the present application provides a wind turbine blade, comprising the wind turbine blade skin provided by the third aspect of the present application.

[0030] The polyester core material of the present application includes modified polyester, wherein the modified polyester material uses a component including the chain segment shown in the above formula 1 (for example, a degradation product of bisphenol A diglycidyl ether containing terminal hydroxyl groups obtained by hydrolyzing the wind turbine blade pultrusion resin) to replace part of ethylene glycol, and a component including the chain segment shown in the above formula 4 (for example, methyltetrahydrophthalic acid containing carboxyl groups obtained by hydrolyzing the wind turbine blade pultrusion resin) to replace part of terephthalic acid, and the chain segments shown in the above formula 1 and the above formula 4 are introduced into the PET material (the chain segments shown in formula 2 and formula 3) through the condensation reaction of hydroxyl and carboxyl groups, so that a higher content of rigid structure groups and a larger spatial internal resistance can be introduced into the PET material, which can make it difficult for the modified polyester molecules to move, so as to simultaneously improve the heat resistance and mechanical properties of PET.

[0031] Furthermore, the present application controls the molar ratio of the chain segments shown in Formula 1 and Formula 2 to be 1:(10-50), so that the PET material is not easily degraded, and its number average molecular weight, molecular weight distribution, and hydroxyl value are within a suitable range, thereby improving the problems of decreased number average molecular weight, wider molecular weight distribution, and decreased viscosity of the PET material, while improving the heat resistance and mechanical properties of PET. DETAILED DESCRIPTION

[0032] In order to make the invention purpose, technical scheme and beneficial technical effect of the present application clearer, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the embodiments described in this specification are only for explaining the present application, not for limiting the present application.

[0033] For simplicity, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form an unambiguous range; and any lower limit can be combined with other lower limits to form an unambiguous range, and any upper limit can be combined with any other upper limit to form an unambiguous range. In addition, although not explicitly stated, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unambiguous range.

[0034] In the description herein, when a composition is described as containing, comprising or including specific components, or when a process is described as containing, comprising or including specific process steps, it is expected that the composition of the present application also consists essentially of or consists of the components, and the process of the present application also consists essentially of or consists of the process steps.

[0035] The use of the terms "including," "comprising," "containing," and "having" should generally be interpreted as open ended and non-limiting unless expressly stated otherwise.

[0036] In the description of this article, it should be noted that, unless otherwise specified, “above” and “below” are inclusive of the number itself, and the “multiple” in “one or more” means more than two.

[0037] The above-mentioned summary of the invention of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of examples, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0038] The inventors have found that the performance of PET can be improved by increasing the molecular weight of PET, such as by introducing a chain extender to increase the diversification of the branched chains, or by adding other resins or functional additives. However, the modification effect of these methods is limited, and since the chain extension is usually performed on the molecular weight of the original PET, it is easy to cause its molecular weight distribution to be too large, at least 3 or 4 or more. The large molecular weight distribution of PET materials will cause the viscosity of the polyester material to be high and the glass transition temperature to be low, resulting in limited improvement in its mechanical properties and heat resistance.

[0039] In view of this, the present application provides a polyester core material and a preparation method thereof, a wind turbine blade skin and a wind turbine blade, aiming to simultaneously improve the heat resistance and mechanical properties of the PET core material.

[0040] In the embodiment of the first aspect of the present application, a polyester core material is provided, comprising a modified polyester, wherein the modified polyester comprises segments shown in the following formulas 1, 2, 3 and 4:

[0041]

[0042] The chain segment of formula 1 is connected to the chain segment of formula 3 or formula 4; the chain segment of formula 4 is connected to the chain segment of formula 1 or formula 2; the molar ratio of the chain segments of formula 1 to formula 2 is 1:(10-50).

[0043] The polyester core material of the present application includes a modified polyester and a foaming agent, wherein the modified polyester material uses a component including a chain segment shown in the above formula 1 (for example, a degradation product of bisphenol A diglycidyl ether containing terminal hydroxyl groups obtained by hydrolyzing a wind turbine blade pultrusion resin) to replace part of ethylene glycol, and a component including a chain segment shown in the above formula 4 (for example, methyltetrahydrophthalic acid containing carboxyl groups obtained by hydrolyzing a wind turbine blade pultrusion resin) to replace part of terephthalic acid, and the chain segments shown in the above formulas 1 and 4 are introduced into the PET material (the chain segments shown in formulas 2 and 3) through the condensation reaction of hydroxyl groups and carboxyl groups, so that a higher content of rigid structure groups and a larger spatial internal resistance can be introduced into the PET material, which can make it difficult for the modified polyester molecules to move, so as to simultaneously improve the heat resistance and mechanical properties of PET.

[0044] Furthermore, the present application controls the molar ratio of the chain segments shown in Formula 1 and Formula 2 to be 1:(10-50), so that the PET material is not easily degraded, and its number average molecular weight, molecular weight distribution, and hydroxyl value are within a suitable range, thereby improving the problems of decreased number average molecular weight, wider molecular weight distribution, and decreased viscosity of the PET material, while improving the heat resistance and mechanical properties of PET.

[0045] Moreover, the present application is a modification performed at the front end of the preparation of PET materials, and partially replaces ethylene glycol and phthalic acid to avoid chain extension on the original PET molecular weight, which leads to a large molecular weight distribution, thereby better improving the heat resistance and mechanical properties of PET. For example, there is a method of modifying the back end after the preparation of PET materials, which is likely to cause a large molecular weight distribution, and the mechanical properties and thermal stability of PET materials are often not achieved at the same time, and the improvement effect is limited.

[0046] At the same time, since the present application introduces a plurality of benzene rings with hydrophobic groups, the water resistance of the modified PET material can be enhanced to improve the comprehensive performance of the PET resin.

[0047] For example, the chain segments shown in Formula 1, Formula 2, Formula 3 and Formula 4 in the modified polyester can be connected in a manner that is one or more of Formula 1-Formula 3-Formula 2-Formula 4, Formula 1-Formula 3-Formula 4-Formula 2, Formula 1-Formula 4-Formula 3-Formula 2, Formula 1-Formula 4-Formula 2-Formula 3, Formula 1-Formula 3-Formula 1-Formula 4-Formula 2, Formula 1-Formula 3-Formula 2-Formula 3-Formula 4 and Formula 2-Formula 4-Formula 2-Formula 3-Formula 1-Formula 3. For example, the reaction formula of the modified polyester can be as follows

[0048] As shown in formula 5.

[0049]

[0050] The raw materials of the chain segments represented by Formula 1, Formula 2, Formula 3 and Formula 4 in the polyester core material in the present application may be from recycled wind turbine blade related materials, such as wind turbine blade pultruded plates, wind turbine blade skins, or may be from other materials.

[0051] For example, the substances including the chain segments shown in the above formula 1 and the above formula 4 in the polyester material of the present application can all be derived from degradation products of thermosetting resin in recycled wind turbine blade pultruded plates. For example, they can be derived from degradation products of bisphenol A diglycidyl ether containing terminal hydroxyl groups and methyltetrahydrophthalic acid in the degradation products.

[0052] Vigorously developing renewable energy, reducing fossil energy consumption, and building a green and low-carbon energy system are important measures to control global warming and achieve carbon reduction targets. As the key core component of wind turbines to capture wind energy, wind turbine blades are leading wind turbines towards high power and large-scale development. Among them, wind turbine blade pultruded plates usually use continuous fibers (such as glass fibers, carbon fibers) as reinforcing materials. Through resin matrix impregnation, higher mechanical properties are obtained than vacuum infusion molding processes, especially the compression performance in the 0° direction can be increased by nearly doubled. The application of pultruded plates makes the design and manufacture of ultra-large wind turbine blades possible.

[0053] Pultruded boards are usually made of thermosetting resin and glass fiber or carbon fiber yarn through pultrusion process. There are literature reports [Dissolution of epoxy thermosets via mild alcoholysis: the mechanism and kinetics study.], [Recycling of Epoxy Thermoset and Composites via GoodSolvent Assisted and Small Molecules Participated Exchange Reactions], [Bonafide upcycling strategy of anhydride cured epoxy and reutilization of decomposed dual monomers into multipurpose applications, Lin Shao, Yu-Chung Chang, Baoming Zhao, Xinyan Yan, Brian J. Bliss, Ming-en Fei, Chenhao Yu, Jinwen Zhang, Chemical Engineering Journal, Volume 464, 2023, 142735], using alkaline hydrolysis method can degrade anhydride cured epoxy resin with similar structure to pultruded resin, and in principle, the separation of fiber and resin in pultruded board can be achieved. However, the high-value utilization of the degradation products of wind turbine blade plates, such as bisphenol A diglycidyl ether and methyltetrahydrophthalic acid, is a technical bottleneck for the application of this technology. Therefore, the development of high-value application scenarios for pultruded board degradation resin products is a key issue facing the alkaline hydrolysis degradation solution of pultruded boards.

[0054] The inventors analyzed that the degradation products of wind turbine blade pultruded sheets, including degradation products of bisphenol A diglycidyl ether and methyltetrahydrophthalic acid, have not been utilized in a high-value manner because: 1) wind turbine blade pultruded sheets currently belong to a relatively cutting-edge technical field, and the degradation of wind turbine blade pultruded sheets is even more cutting-edge, and the cost of degrading wind turbine blade pultruded sheets is high, and the economy is poor, resulting in less research data; 2) the content of epoxy resin in wind turbine blade pultruded sheets is relatively low, with a mass content of only about 10% to 20%, which is difficult to be utilized in a high-value manner; 3) the composition of the degradation products of wind turbine blade pultruded sheets is complex, and it is difficult to find a suitable parameter and range or standard to evaluate whether they can be utilized; 4) due to the complexity of the degradation products and the almost no previous research data, whether adding them to other materials can generate application value is a blank technical field and is difficult.

[0055] The present application overcomes the defect that the degradation products of thermosetting resin in wind turbine blade pultruded plates are difficult to be utilized in a high-value manner by controlling the hydroxyl value of the degradation products of the wind turbine blade pultruded plates within a suitable range, for example, 300 mg KOH / g to 400 mg KOH / g. The degradation products of bisphenol A diglycidyl ether and methyltetrahydrophthalic acid, which are the degradation products of thermosetting resin in the wind turbine blade pultruded plates, are successfully introduced into PET materials, and the wind turbine blade pultruded plates are combined with PET materials for application, which not only realizes the high-value application of the degradation products of the wind turbine blade pultruded plates, but also comprehensively improves the performance of the PET material, for example, the heat resistance and mechanical strength of the PET material are improved at the same time, and the application value is high.

[0056] Furthermore, the present application can control the amount of bisphenol A diglycidyl ether degradation products and methyltetrahydrophthalic acid introduced, for example, the percentage of the weight of the segments contained therein to the total weight of the modified PET material is within a suitable range, for example, the molar ratio of the segments shown in Formula 4 to Formula 3, the ratio of the total molar amount of the segments shown in Formulas 1 and 2 to the total molar amount of the segments shown in Formulas 3 and 4, so as to affect the terminal carboxyl content and the ester group content in the modified polyester, so that the contents of the two are lower, thereby further improving the mechanical properties, thermal stability and water resistance of PET.

[0057] For example, in some embodiments, the modified polyester satisfies at least one of the following conditions:

[0058] a. The molar ratio of the chain segments represented by formula 4 to formula 3 is 1:(10-50);

[0059] b. The ratio of the total molar amount of the segments represented by Formula 1 and Formula 2 to the total molar amount of the segments represented by Formula 3 and Formula 4 is 1:(0.6-2), and may be 1:(1.0-1.5);

[0060] c. The weight of the chain segments represented by Formula 1 and Formula 4 accounts for 1% to 20% of the total weight of the modified polyester.

[0061] In the present application, the PET material is modified at the front end, and the number average molecular weight of the modified PET material is 20000Da to 30000Da, and the molecular weight distribution is small, which can be 1.5 to 2.2. The small hydroxyl value can make the heat resistance and mechanical properties of the modified polyester more excellent, such as tensile strength and yield strength. In addition, the water resistance, curing speed, hardness and mechanical properties of the PET material can also be improved.

[0062] For example, in some embodiments, the modified polyester satisfies at least one of the following conditions:

[0063] d. The number average molecular weight of the modified polyester is 20000Da to 30000Da, and can be 25000Da to 29000Da;

[0064] e. The molecular weight distribution of the modified polyester is 1.5 to 2.2;

[0065] f. The hydroxyl value of the modified polyester is 50 mgKOH / g to 150 mgKOH / g.

[0066] The modified PET material of the present application has excellent heat resistance. For example, in some embodiments, the melt viscosity of the modified polyester is 250 Pa·s to 520 Pa·s; and / or the heat deformation temperature of the modified polyester is 100°C to 120°C, optionally 109°C to 120°C.

[0067] The modified PET material of the present application not only has excellent heat resistance, but also has high mechanical strength. For example, in some embodiments, the ultimate tensile strength of the modified polyester is 40MPa to 55MPa, optionally 43MPa to 55MPa; and / or, the yield strength of the modified polyester is 35MPa to 50MPa, optionally 36MPa to 50MPa.

[0068] In some embodiments, the polyester core material further includes a foaming agent, and the mass ratio of the modified polyester to the foaming agent is 1:(0.2-0.8); optionally, the foaming agent includes one or more of azodicarbonamide, azobisisobutyronitrile and azodiacetate.

[0069] In an embodiment of the second aspect of the present application, a method for preparing the polyester core material provided in the first aspect of the present application is provided, comprising:

[0070] Providing degradation products of a wind turbine blade pultruded plate, wherein the degradation products of the wind turbine blade pultruded plate respectively include components of structures shown in Formula 1 and Formula 4;

[0071] The degradation product of the wind turbine blade pultruded sheet is mixed with terephthalic acid and ethylene glycol to obtain a modified polyester;

[0072] The modified polyester and the foaming agent are mixed and expanded to obtain a polyester core material.

[0073] The inventors have discovered that when the hydroxyl value of the degradation products of the wind turbine blade pultruded sheet is controlled within a certain range, such as 300 mg KOH / g to 400 mg KOH / g, the degradation products of the thermosetting resin in the wind turbine blade pultruded sheet, such as bisphenol A diglycidyl ether degradation products and methyltetrahydrophthalic acid, can be introduced into the PET material to improve the heat resistance and mechanical strength of the PET material, thereby realizing the high-value application of the degradation products of the wind turbine blade pultruded sheet.

[0074] In some embodiments, in the step of providing a degradation product of a wind turbine blade pultruded plate, wherein the degradation product of the wind turbine blade pultruded plate includes components having structures represented by Formula 1 and Formula 4, respectively, the hydroxyl value of the degradation product of the wind turbine blade pultruded plate is 300 mg KOH / g to 400 mg KOH / g.

[0075] In some embodiments, the step of mixing the degradation product of the wind turbine blade pultruded sheet with terephthalic acid and ethylene glycol to obtain the modified polyester includes subjecting the degradation product of the wind turbine blade pultruded sheet to a condensation reaction with terephthalic acid and ethylene glycol in an inert atmosphere and a vacuum degree of 0Pa to 10Pa at 240°C to 300°C for 5h to 12h to obtain the modified polyester.

[0076] In some embodiments, the step of mixing the modified polyester and the foaming agent and expanding them to obtain the polyester core material includes mixing and stirring the modified polyester and the foaming agent in a mass ratio of 1:(0.2-0.8), stirring for 2h-10h in a nitrogen atmosphere at 240°C-260°C, and cooling to room temperature to fix the shape to obtain the PET core material.

[0077] In an embodiment of the third aspect of the present application, a wind turbine blade skin is provided, comprising the polyester core material provided in the first aspect of the present application.

[0078] In an implementation of the fourth aspect of the present application, a wind turbine blade skin is provided, comprising the wind turbine blade skin provided by the third aspect of the present application.

[0079] The present application can first obtain degradation products by degrading discarded wind turbine blade pultruded plates, then control the hydroxyl value of the degradation products within a certain range, and apply the degradation products of the wind turbine blade pultruded plates to PET for high value, so as to obtain a PET core material with excellent heat resistance and mechanical properties. The PET core material can then be prepared into a wind turbine blade skin, and the wind turbine blade skin can be further assembled into a wind turbine blade, thus realizing the long-term recycling of wind turbine blade materials and effectively integrating the resources of wind turbine blades. This is of great significance to environmental protection, production costs, and resource utilization, and is conducive to sustainable development.

[0080] Example

[0081] The following examples more specifically describe the disclosure of the present application, which are intended for illustrative purposes only, as it will be apparent to those skilled in the art that various modifications and variations are possible within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0082] Example 1

[0083] The present embodiment provides a method for preparing a modified PET core material, comprising: obtaining degradation products of a wind turbine blade pultruded plate having a hydroxyl value of ˜350 mg KOH / g, wherein the degradation products include degradation products of bisphenol A diglycidyl ether and methyltetrahydrophthalic acid, and subjecting the degradation products of the wind turbine blade pultruded plate to a condensation reaction with terephthalic acid and ethylene glycol in an inert atmosphere and a vacuum degree of 10 Pa at 300° C. for 5 hours to obtain a modified PET resin.

[0084] The molar ratio of bisphenol A diglycidyl ether to ethylene glycol is controlled to be 1:30, the molar ratio of methyltetrahydrophthalic acid to terephthalic acid is controlled to be 1:25, the ratio of the total molar amount of bisphenol A diglycidyl ether and ethylene glycol to the total molar amount of methyltetrahydrophthalic acid and terephthalic acid is 1:1, and the weight of bisphenol A diglycidyl ether and methyltetrahydrophthalic acid accounts for 8% of the total weight of the modified PET resin.

[0085] The modified PET resin and azodicarbonamide were mixed at a mass ratio of 1:0.5, stirred for 4 hours at 250° C. in a nitrogen atmosphere, and cooled to room temperature to fix the mixture, so as to obtain a PET core material.

[0086] Embodiments 2 to 8

[0087] Example 2, compared with Example 1, the main difference is that the molar ratio of methyltetrahydrophthalic acid to terephthalic acid is changed to 1:50, other conditions such as the molar ratio of bisphenol A diglycidyl ether to ethylene glycol is 1:30, the ratio of the total molar amount of bisphenol A diglycidyl ether and ethylene glycol to the total molar amount of methyltetrahydrophthalic acid and terephthalic acid is 1:1, and the weight percentage of bisphenol A diglycidyl ether and methyltetrahydrophthalic acid to the total weight of the modified PET resin is adaptively adjusted.

[0088] Example 3, compared with Example 1, the main difference is that the molar ratio of methyltetrahydrophthalic acid to terephthalic acid is changed to 1:10, other conditions such as the molar ratio of bisphenol A diglycidyl ether to ethylene glycol is 1:30, the ratio of the total molar amount of bisphenol A diglycidyl ether and ethylene glycol to the total molar amount of methyltetrahydrophthalic acid and terephthalic acid is 1:1, and the weight percentage of bisphenol A diglycidyl ether and methyltetrahydrophthalic acid to the total weight of the modified PET resin is adaptively adjusted.

[0089] Example 4, compared with Example 1, the main difference is that the weight of bisphenol A diglycidyl ether and methyltetrahydrophthalic acid is changed to 20% of the total weight of the modified polyester, and other conditions such as the molar ratio of bisphenol A diglycidyl ether to ethylene glycol is 1:30, the ratio of the total molar amount of bisphenol A diglycidyl ether and ethylene glycol to the total molar amount of methyltetrahydrophthalic acid and terephthalic acid is 1:1, and the molar ratio of methyltetrahydrophthalic acid to terephthalic acid is adaptively adjusted.

[0090] Example 5, compared with Example 1, the main difference is that the ratio of the total molar amount of bisphenol A diglycidyl ether and ethylene glycol to the total molar amount of methyltetrahydrophthalic acid and terephthalic acid is changed to 1:1.5, and the other conditions are that the molar ratio of bisphenol A diglycidyl ether to ethylene glycol is 1:30, the molar ratio of methyltetrahydrophthalic acid to terephthalic acid is 1:25, and the percentage of the weight of bisphenol A diglycidyl ether and methyltetrahydrophthalic acid to the total weight of the modified PET resin is adaptively changed.

[0091] Example 6, compared with Example 1, the main difference is that the ratio of the total molar amount of bisphenol A diglycidyl ether and ethylene glycol to the total molar amount of methyltetrahydrophthalic acid and terephthalic acid is changed to 1:0.67, and the other conditions are that the molar ratio of bisphenol A diglycidyl ether to ethylene glycol is 1:30, the molar ratio of methyltetrahydrophthalic acid to terephthalic acid is 1:25, and the percentage of the weight of bisphenol A diglycidyl ether and methyltetrahydrophthalic acid to the total weight of the modified PET resin is adaptively changed.

[0092] Example 7, compared with Example 1, is mainly different in that the degradation product of the wind turbine blade pultruded plate having a hydroxyl value of ˜500 mg KOH / g is used in the preparation method.

[0093] Example 8, compared with Example 1, is mainly different in that, in the preparation method, commercial PET pellets are used to replace terephthalic acid and ethylene glycol, and then degradation products of wind turbine blade pultruded plates with a hydroxyl value of ~350 mg KOH / g are added for modification to obtain modified PET material.

[0094] Comparative Examples 1 to 3

[0095] Comparative Example 1 is mainly different from Example 1 in that only the chain segment shown in Formula 1 and only bisphenol A diglycidyl ether are introduced into the modified PET resin.

[0096] Comparative Example 2, compared with Example 1, is mainly different in that the modified PET resin only introduces the chain segment shown in Formula 4 and only introduces methyltetrahydrophthalic acid.

[0097] Comparative Example 3, compared with Example 1, is mainly different in that the molar ratio of bisphenol A diglycidyl ether to ethylene glycol in the modified PET resin is changed to 1:55, the molar ratio of methyltetrahydrophthalic acid to terephthalic acid under other conditions is 1:25, the ratio of the total molar amount of bisphenol A diglycidyl ether and ethylene glycol to the total molar amount of methyltetrahydrophthalic acid and terephthalic acid is 1:1, and the mass percentage of the weight of bisphenol A diglycidyl ether and methyltetrahydrophthalic acid to the total weight of the modified PET resin is adaptively changed.

[0098] The properties of the modified PET resins prepared in the examples and comparative examples were tested, and the test results are shown in Tables 1-2 below.

[0099] Measurement method

[0100] Number average molecular weight: according to ASTM D5296 / ASTM D6226 standards.

[0101] Molecular weight distribution: refer to ASTM D5296 / ASTM D6226 standards.

[0102] Hydroxyl value: refer to ASTM D4274 standard.

[0103] Melt viscosity: measured in accordance with ASTM D3835 / ISO 11443.

[0104] Heat deformation temperature: refer to ASTM D648 standard.

[0105] Ultimate tensile strength: Refer to ISO 527 standard.

[0106] Yield strength: Refer to ISO 527 standard.

[0107] Table 1 Physical and chemical properties test data of PET resin in various embodiments and comparative examples

[0108]

[0109]

[0110] Table 2 Test data of heat resistance and mechanical properties of PET resin in various embodiments and comparative examples

[0111]

[0112] As can be seen from Tables 1 to 2, the modified PET resin of the present application example obtains samples with excellent heat resistance and mechanical properties by introducing the segments shown in Formula 1 and Formula 4 and controlling the proportion of the introduced amounts. Among them, Comparative Examples 1 to 2 do not introduce the segments shown in Formula 1 and Formula 2 at the same time, and the heat resistance and mechanical strength are reduced, especially the heat deformation temperature, ultimate tensile strength and yield strength. Although Comparative Example 3 introduces the segments shown in Formula 1 and Formula 2, the introduction amount of the segments shown in Formula 1 is small, and the ethylene glycol is more, which may lead to poor polymerization reaction of PET materials, decreased number average molecular weight, increased molecular distribution, and significantly decreased heat resistance and mechanical properties, indicating that the introduction of the segments shown in Formula 1 and Formula 4 and the proportion of the introduced amounts are very important for improving the heat resistance and mechanical properties of the modified PET resin.

[0113] In addition, the inventors have also found through experimental research that the amount of the chain segments shown in Formula 4, the total amount of the chain segments shown in Formula 1 and Formula 4, the total amount of the chain segments shown in Formula 1 and Formula 2 and the total amount of the chain segments shown in Formula 3 and Formula 4 can be controlled to further improve the heat resistance and mechanical properties of PET. From Examples 1 to 3, it can be seen that the increase in the amount of the chain segments shown in Formula 4 can increase the rigid groups in the polymer molecular structure, and improve the heat resistance and mechanical properties. From Examples 1, 4 to 6, it can be seen that the proportion of the total amount of the chain segments shown in Formula 1 and Formula 4 can be controlled, the total amount of the chain segments shown in Formula 1 and Formula 2 and the total amount of the chain segments shown in Formula 3 and Formula 4 can be controlled in a suitable range, the number average molecular weight, molecular weight distribution and hydroxyl value of the modified polyester can be controlled in a suitable range, the number average molecular weight can be increased, the molecular weight distribution can be reduced, and the performance of PET can be further improved.

Claims

1. A polyester core material, characterized in that: The polyester core material includes modified polyester, wherein the modified polyester includes segments shown in the following formulas 1, 2, 3 and 4: The segment represented by Formula 1 is connected to the segment represented by Formula 3 or Formula 4; the segment represented by Formula 4 is connected to the segment represented by Formula 1 or Formula 2; The molar ratio of the chain segments represented by Formula 1 to those represented by Formula 2 is 1:(10-50).

2. The polyester core material according to claim 1, characterized in that: The modified polyester meets at least one of the following characteristics: a. The molar ratio of the chain segment represented by formula 4 to that represented by formula 3 is 1:(10 to 50); b. The ratio of the total molar amount of the segments represented by the formula 1 and the formula 2 to the total molar amount of the segments represented by the formula 3 and the formula 4 is 1:(0.6-2), and may be 1:(1.0-1.5); c. The weight of the chain segments represented by Formula 1 and Formula 4 accounts for 1% to 20% of the total weight of the modified polyester.

3. The polyester core material according to claim 1, characterized in that: The modified polyester meets at least one of the following characteristics: d. The number average molecular weight of the modified polyester is 20000Da to 30000Da; e. The molecular weight distribution of the modified polyester is 1.5 to 2.2; f. The hydroxyl value of the modified polyester is 50 mgKOH / g to 150 mgKOH / g.

4. The polyester core material according to claim 1, characterized in that: The melt viscosity of the modified polyester is 250 Pa·s to 520 Pa·s; and / or the heat deformation temperature of the modified polyester is 100° C. to 120° C.

5. The polyester core material according to claim 1, characterized in that: The ultimate tensile strength of the modified polyester is 40 MPa to 55 MPa; and / or the yield strength of the modified polyester is 35 MPa to 50 MPa.

6. The polyester core material according to claim 1, characterized in that: The polyester core material also includes a foaming agent, and the mass ratio of the modified polyester to the foaming agent is 1:(0.2-0.8); optionally, the foaming agent includes one or more of azodicarbonamide, azobisisobutyronitrile and azodiacetate.

7. The method for preparing a polyester core material according to any one of claims 1 to 6, characterized in that: include: Providing a degradation product of a wind turbine blade pultruded plate, wherein the degradation product of the wind turbine blade pultruded plate comprises components of the chain segments represented by Formula 1 and Formula 4; The degradation product of the wind turbine blade pultruded plate is mixed with terephthalic acid and ethylene glycol to react to obtain a modified polyester; The modified polyester and a foaming agent are mixed and expanded to obtain the polyester core material.

8. The method for preparing a polyester core material according to claim 7, characterized in that: In the step of providing a degradation product of a wind turbine blade pultruded plate, wherein the degradation product of the wind turbine blade pultruded plate includes components of the chain segments represented by Formula 1 and Formula 4, the hydroxyl value of the degradation product of the wind turbine blade pultruded plate is 300 mg KOH / g to 400 mg KOH / g.

9. The method for preparing a polyester core material according to claim 7, characterized in that: The step of mixing the degradation product of the wind turbine blade pultruded sheet with terephthalic acid and ethylene glycol to obtain the modified polyester includes reacting the degradation product of the wind turbine blade pultruded sheet with terephthalic acid and ethylene glycol in an inert atmosphere and a vacuum degree of 0Pa to 10Pa at 240°C to 300°C for 5h to 12h to obtain the modified polyester.

10. The method for preparing a polyester core material according to claim 7, characterized in that: The step of mixing the modified polyester and the foaming agent and expanding them to obtain the polyester core material includes mixing and stirring the modified polyester and the foaming agent in a mass ratio of 1:(0.2-0.8), stirring for 2h-10h in a nitrogen atmosphere at 240°C-260°C, and cooling to room temperature to set the shape to obtain the polyester core material.

11. A wind turbine blade skin, characterized in that: The invention comprises the polyester core material as claimed in any one of claims 1 to 6.

12. A wind turbine blade, characterized in that: It comprises the wind turbine blade skin as claimed in claim 11.

Citation Information

Patent Citations

  • Shape memory epoxy resin and preparation method thereof

    CN104744893A

  • Multilobal profiled polyethylene terephthalate fiber FDY (fully-drawn yarn) and preparation method thereof

    CN106811821A

  • Modified polyester polyol, preparation method and applications thereof

    CN109553766A

  • Epoxy resin and process for making the same

    CN1437625A

  • Production of polyester resin having epoxy group

    JP1984197426A

Cited By

  • Polyester core material and preparation method therefor, wind turbine blade skin and wind turbine blade

    WO2026061112A1