Preparation of starch-based adhesive with strong adhesive strength and capability of resisting hot water soaking and application of starch-based adhesive in wood processing
The starch is treated by high amylose, low concentration alkali liquid and calcium chloride, and urea formaldehyde resin and glutaraldehyde are added to form a composite adhesive, which solves the problem of structural disintegration of starch-based adhesive in hot water at 60℃, and achieves high temperature Good adhesion and simple process to meet national standards for starch-based adhesive applications.
Patent Information
- Application Number
- CN202411181866.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
AI Technical Summary
The existing starch-based adhesives are difficult to maintain a dense three-dimensional network structure in hot water of 60°C, and cannot meet the latest national standards for the hot water immersion requirements of artificial boards. At the same time, the modification reaction is complex and the synthesis is difficult, which limits its application.
The starch is treated with high amylose, low-concentration alkali solution and low-concentration calcium chloride solution, adjust the pH to 5.5, add urea formaldehyde resin and glutaraldehyde as curing agent to form a composite adhesive, and form a dense structure and urea formaldehyde resin through long amylose winding. The hydrophobic effect of the adhesive enhances the heat-resistant water performance.
The prepared starch-based adhesive can maintain good adhesion in room temperature water and 60℃ hot water, meet the requirements of the national standard GB/T 17657-2022, and has a simple process and is suitable for a wide range of wood processing applications.
Smart Images

Figure CN118956293A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wood adhesives, and in particular relates to the preparation of a starch-based adhesive which has strong bonding force and can withstand hot water immersion, and its application in wood processing. Background Art
[0002] In the wood processing industry, traditional adhesives such as urea-formaldehyde resins, phenolic resins and polyurethanes are mainly derived from fossil fuels. These adhesives have excellent performance and can maintain excellent adhesion even in humid or water-soaked environments, so they are widely used in the production of plywood, particleboard and medium-density fiberboard. However, these adhesives will inevitably release harmful gases such as formaldehyde during the synthesis and use process, posing a potential threat to human health. In view of this, the development of green and environmentally friendly bio-based (such as protein, tannin, lignin, chitosan and starch) adhesives has attracted increasing attention.
[0003] Among many bio-based adhesives, starch stands out due to its low price. Starch is rich in hydroxyl groups and can form hydrogen bonds with cellulose on the surface of wood, thereby achieving the bonding of wood boards. However, the polyhydroxyl properties of starch also make it highly hydrophilic, which leads to a sharp weakening of the bonding ability of starch-based adhesives whether it is soaked in water or in a humid environment for a long time, thus greatly restricting its application range.
[0004] In order to improve the water resistance of starch, it is currently mainly achieved by modifying starch. On the one hand, by introducing hydrophobic groups (such as oxidation, esterification, etc.) into the starch chain to reduce hydroxyl groups, thereby reducing its hydrophilicity; on the other hand, by using covalent bonds or non-covalent interactions (such as grafting, cross-linking, etc.), the starch chain forms a dense three-dimensional network, thereby reducing the penetration rate of water into the network. Through the above methods, although starch-based wood adhesives that can withstand immersion in water at room temperature have been successfully developed. However, the latest national standard GB / T 17657-2022 has put forward higher requirements for artificial boards, that is, artificial plywood must not only be able to withstand immersion in water at room temperature, but also must be able to withstand immersion in hot water at 60°C. However, since the kinetic energy of starch chains in 60°C hot water is significantly enhanced, it is difficult to maintain the original dense three-dimensional network structure, so most starch-based adhesives cannot meet this requirement. For example, the applicant's previous invention patent CN115340832A used high-amylose starch and urea-formaldehyde resin as raw materials to prepare a starch-based water-resistant flame-retardant adhesive. Although the ability of the starch-based adhesive to resist water immersion has been improved to a certain extent, when immersed in hot water, due to the high ambient temperature and strong molecular mobility, the dense three-dimensional network structure formed by the entanglement of starch chains disintegrates. In addition, in order to gelatinize high-amylose starch, a high-concentration calcium chloride solution is used, but calcium chloride itself is very easy to absorb water, resulting in it being unable to withstand immersion in 60°C hot water. In addition, although a few researchers have developed starch-based adhesives that can withstand hot water immersion, there are problems such as complex modification reactions and difficulty in synthesis, resulting in unsatisfactory actual application effects. For example, LI et al. used starch and citric acid to generate an esterified cross-linked product for plywood, which can withstand hot water immersion. The reaction temperature is 100°C and the time is 1 hour. When using it, the glue needs to be coated on the wood board, and then hot-pressed at 200°C and 1.0 MPa for 6 minutes to obtain hot water-resistant plywood (LI C, HOU D, LEI H, et al. Effective and eco-friendly safe self-antimildew strategy to simultaneously improve the water resistance and bonding strength of starch-based adhesive [J]. International Journal of Biological Macromolecules, 2023, 248: 125889.). However, although this method can make plywood withstand hot water immersion, the modification method is complicated and the synthesis is difficult, which is not conducive to promotion and application.
[0005] In summary, it is necessary to develop starch-based adhesives with strong bonding strength and the ability to withstand 60°C hot water immersion for wood processing. Summary of the invention
[0006] In order to overcome the above-mentioned deficiencies of the prior art, the present invention proposes a method for preparing a starch-based adhesive. The starch-based adhesive prepared by the method of the present invention, when used in combination with a curing agent, not only has strong bonding strength, but also can maintain good bonding strength after being immersed in room temperature water or hot water for a long time.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] The present invention provides an application of a starch-based adhesive in wood processing, specifically: the starch-based adhesive is evenly coated on the surface of a wooden board, a curing agent is added, and the wooden board is pressed and dried, so that the wooden board can be firmly bonded by the starch-based adhesive, and even if the wooden board is immersed in room temperature water or 60°C hot water for a long time, the adhesive can still provide good bonding strength;
[0009] The preparation method of the starch-based adhesive comprises the following steps:
[0010] S1, soaking high-amylose starch with low-concentration alkali solution to obtain starch emulsion;
[0011] S2, adding a low concentration calcium chloride solution to the starch emulsion, adjusting the pH value of the mixed system to below 5.5, and then heating to form a starch paste;
[0012] S3. Add urea-formaldehyde resin dissolved in water into starch paste, heat and mix evenly to obtain starch-based adhesive.
[0013] Preferably, the curing agent is glutaraldehyde, and the amount of the curing agent is no more than 10% of the mass of the starch-based adhesive.
[0014] Preferably, in S3, the amount of urea-formaldehyde resin used accounts for 10%-30% of the mass of the starch paste.
[0015] If the content of amylose chains is too high, the starch adhesive will become viscous and difficult to apply. Even if the adhesive is applied to the wooden board, its permeability into the micropores on the surface of the wooden board is poor, so the bonding performance deteriorates.
[0016] Preferably, the high-amylose starch refers to natural starch with an amylose content of 50%-60% in starch granules.
[0017] Preferably, the low concentration alkali solution in S1 is a NaOH solution with a mass concentration of 0.5-1.5%, and the low concentration calcium chloride solution in S2 is a calcium chloride solution with a mass concentration of 3-5%.
[0018] Urea-formaldehyde resin is the most widely used adhesive in wood, but after it is directly compounded with ordinary starch glue, the water resistance of the composite glue is very poor. This is mainly because ordinary starch glue contains a large amount of branched starch molecules, and the glucan polymerization degree of branched starch is high, the molecular weight is huge, and the hydroxyl density is high, so it is highly hydrophilic and easy to absorb moisture, which destroys the continuous and dense hydrophobic structure of urea-formaldehyde resin, resulting in poor water resistance of the composite glue. For this reason, the present invention uses high-amylose starch to replace ordinary starch, and adopts low-concentration alkali (0.5-1.5% concentration alkali solution) and low-concentration (3-5% concentration calcium chloride solution) solution to gelatinize the high-amylose starch, and then adds urea-formaldehyde resin to it to make high-amylose starch / urea-formaldehyde resin composite glue. The adhesive only needs to add a very small amount of urea-formaldehyde resin to the starch glue (the amount can be as low as 10% of the mass of the starch glue), and use it with a small amount of glutaraldehyde (no more than 10% of the mass of the adhesive) curing agent, so that the composite glue can have good hot water resistance. The main reason is that in the starch-based adhesive prepared by the above method, the long-chain amylose molecules are entangled with each other to form a dense structure, and the hydroxyl groups are embedded in the structure, so the hydrophilicity is weak; and the urea-formaldehyde resin molecules are also easy to form a dense structure through hydrophobic action, and the interaction between urea-formaldehyde resin and wood fiber is strong. Therefore, after the composite glue is applied to the wood board, the urea-formaldehyde resin mainly gathers at the interface between the glue and the wood board, and forms a water-blocking layer after curing, thereby hindering the water absorption of the starch chain, so that the composite glue has good moisture-proof and water-resistant stability. At the same time, the hydrogen bonds between glutaraldehyde and starch molecules are cross-linked, strengthening the network structure inside the colloid, further reducing the hydrophilicity of the colloid, and improving its hot water resistance.
[0019] Preferably, the mass ratio of the high amylose starch to the low concentration alkali solution in S1 is 1-2:3, and the mass ratio of the low concentration calcium chloride solution to the starch emulsion in S2 is 0.3-1:1. The use of the low concentration calcium chloride solution can avoid affecting the water resistance of the starch-based adhesive due to the water absorption of calcium chloride itself.
[0020] Preferably, in S2, the pH value of the mixed system is adjusted to 5.0-5.5. If the pH value is too high, the curing effect of the starch-based adhesive will be affected and the stability of the structure will be reduced.
[0021] Preferably, the heating temperature in S2 is not lower than 95° C., and the heating time is not shorter than 30 min.
[0022] Preferably, the temperature of heating and mixing in S3 is not less than 95°C.
[0023] Preferably, in S3, when dissolved in water, the mass ratio of urea-formaldehyde resin to water is not higher than 1:1.
[0024] Preferably, when the starch-based adhesive is evenly applied on the surfaces of the two wooden boards, the coating amount on each side is not higher than 200 g / m 2 .
[0025] Preferably, the temperature of pressing and drying the wood board is not less than 100° C. and the time is not less than 2 hours.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The present invention discloses a method for preparing a starch-based adhesive, which uses high-amylose starch (amylose content is 50%-60%), low-concentration NaOH solution, low-concentration CaCl2 solution, and urea-formaldehyde resin as raw materials. The high-amylose starch is first soaked in a sodium hydroxide solution for a period of time, and then a calcium chloride solution is added, and the pH value of the system is adjusted to below 5.5, and then the system is heated to a starch paste, and then a water-soluble urea-formaldehyde resin is added to the starch paste to obtain a starch-based adhesive. The starch-based adhesive prepared by the method of the present invention is used in combination with a curing agent. Not only does it have a strong bonding force, but it can also maintain good bonding force after being soaked in room temperature water or hot water for a long time. When it is applied to wood processing, the adhesive is evenly coated on the surface of the wooden board, and then an appropriate amount of curing agent is added, and the wooden board is pressed and dried. The wooden board can be firmly bonded by the starch-based adhesive. Even if it is soaked in room temperature water or 60°C hot water for a long time, the adhesive can still provide good bonding force. Specifically, the present invention has the following advantages:
[0028] (1) The starch-based adhesive prepared by the method of the present invention has excellent bonding ability, and after being immersed in room temperature water and 60° C. hot water, it still has good bonding ability, and can meet the use requirements of the national standard GB / T 17657-2022.
[0029] (2) The method for preparing the starch-based adhesive of the present invention has the characteristics of simple process and easy production.
[0030] (3) The starch-based adhesive prepared by the method of the present invention is suitable for the processing of all wood products, can meet the application requirements of wood bonding and wood product processing, and has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is the shear strength of different bonded wood panels at room temperature, after being soaked in water at room temperature for 3 hours, and after being soaked in 60℃ hot water for 3 hours. DETAILED DESCRIPTION
[0032] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0033] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0034] Example 1: Preparation method of a starch-based adhesive and its application in wood processing
[0035] (1) Weigh 0.5 g of sodium hydroxide and add it to 50 mL of water, stir evenly to obtain a NaOH solution; then weigh 30 g of high-amylose starch (amylose content of 55%) and add it to the NaOH solution, stir evenly and let it stand and soak for 12 hours to obtain a starch emulsion.
[0036] (2) Weigh 1.9 g of calcium chloride and add it to 38 mL of water, stir evenly to obtain a CaCl2 solution, then add the obtained CaCl2 solution to the starch emulsion of step (1), stir evenly to obtain a mixed system.
[0037] (3) adding 1 mol / L hydrochloric acid to the mixed system of step (2) to adjust the pH value of the system to 5.5, and then heating to 98° C. while stirring (120 rpm) and heating at this temperature for 30 min to obtain a starch paste.
[0038] (4) Weigh 3 g of urea-formaldehyde resin powder and add it to 3 mL of water. After stirring evenly, add the resulting solution to the starch paste in step (3), and continue stirring at 98° C. for 30 min to obtain a starch-based adhesive.
[0039] (5) Weigh 0.1 g of the starch-based adhesive in step (4) and evenly apply it on the surfaces of two wooden boards, where the coating area of each board is 2.5 cm 2 , coating weight is 200g / m 2 , and then a total of 10 μL (10 mg) of glutaraldehyde was added dropwise to the two coated areas (5 μL per area).
[0040] (6) Align the areas of the two wooden boards coated with the starch-based adhesive in step (5), bond them together, press them tightly, and place them at a constant temperature of 110° C. for curing for 2 hours.
[0041] (7) The bonded wood board obtained in step (6) was divided into three parts, one of which was pulled apart using a mechanical testing machine at room temperature, and its shear strength was measured to be 6.75±0.38MPa. The second part was placed in room temperature water and then soaked for 3 hours and then measured, and its shear strength was measured to be 1.13±0.18MPa. The third part was placed in 60°C hot water and then soaked for 3 hours and then immediately measured, and its shear strength was measured to be 0.85±0.21MPa.
[0042] Example 2: Preparation method of a starch-based adhesive and its application in wood processing
[0043] (1) Weigh 1 g of sodium hydroxide and add it to 100 mL of water, stir it evenly to obtain a NaOH solution; then weigh 66 g of high-amylose starch (amylose content of 55%) and add it to the NaOH solution, stir it evenly and let it stand and soak for 12 hours to obtain a starch emulsion.
[0044] (2) Weigh 5 g of calcium chloride and add it to 95 mL of water, stir evenly to obtain a CaCl2 solution, then add the obtained CaCl2 solution to the starch emulsion of step (1), stir evenly to obtain a mixed system.
[0045] (3) adding 1 mol / L hydrochloric acid to the mixed system of step (2) to adjust the pH value of the system to 5.0, and then heating to 98° C. while stirring (120 rpm), and heating at this temperature for 30 min to obtain a starch paste.
[0046] (4) Weigh 10 g of urea-formaldehyde resin powder and add it to 10 mL of water. After stirring evenly, add the resulting solution to the starch paste in step (3), and continue stirring at 98° C. for 30 min to obtain a starch-based adhesive.
[0047] (5) Weigh 0.1 g of the starch-based adhesive in step (4) and evenly apply it on the surfaces of two wooden boards, where the coating area of each board is 2.5 cm 2 , coating weight is 200g / m 2 , and then a total of 10 μL of glutaraldehyde was added dropwise to the two coated areas (5 μL per area).
[0048] (6) Align the areas of the two wooden boards coated with the starch-based adhesive in step (5), bond them together, press them tightly, and place them at a constant temperature of 110° C. for curing for 2 hours.
[0049] (7) The bonded wood board obtained in step (6) was divided into three parts, one of which was pulled apart using a mechanical testing machine at room temperature, and its shear strength was measured to be 8.24±1.70 MPa. The second part was placed in room temperature water and then soaked for 3 hours and then measured, and its shear strength was measured to be 1.48±0.21 MPa. The third part was placed in 60°C hot water and then soaked for 3 hours and then immediately measured, and its shear strength was measured to be 0.97±0.19 MPa.
[0050] Example 3: Preparation method of a starch-based adhesive and its application in wood processing
[0051] (1) Weigh 0.5 g of sodium hydroxide and add it to 50 mL of water, stir evenly to obtain a NaOH solution; then weigh 30 g of high-amylose starch (amylose content of 55%) and add it to the NaOH solution, stir evenly and let it stand and soak for 12 hours to obtain a starch emulsion.
[0052] (2) Weigh 1.9 g of calcium chloride and add it to 38 mL of water, stir evenly to obtain a CaCl2 solution, then add the obtained CaCl2 solution to the starch emulsion of step (1), stir evenly to obtain a mixed system.
[0053] (3) adding 1 mol / L hydrochloric acid to the mixed system of step (2) to adjust the pH value of the system to 5.5, and then heating to 98° C. while stirring (120 rpm) and heating at this temperature for 30 min to obtain a starch paste.
[0054] (4) Weigh 9 g of urea-formaldehyde resin powder and add it to 10 mL of water. After stirring evenly, add the resulting solution to the starch paste in step (3), and continue stirring at 98° C. for 30 min to obtain a starch-based adhesive.
[0055] (5) Weigh 0.1 g of the starch-based adhesive in step (4) and evenly apply it on the surfaces of two wooden boards, where the coating area of each board is 2.5 cm 2 , coating weight is 200g / m 2 , and then a total of 10 μL of glutaraldehyde was added dropwise to the two coated areas (5 μL per area).
[0056] (6) Align the areas of the two wooden boards coated with the starch-based adhesive in step (5), bond them together, press them tightly, and place them at a constant temperature of 110° C. for curing for 2 hours.
[0057] (7) The bonded wood board obtained in step (6) was divided into three parts, one of which was pulled apart at room temperature using a mechanical testing machine, and its shear strength was measured to be 8.18±1.04MPa. The second part was placed in room temperature water and then soaked for 3 hours and then measured, and its shear strength was measured to be 1.75±0.25MPa. The third part was placed in 60°C hot water and then soaked for 3 hours and then immediately measured, and its shear strength was measured to be 1.34±0.15MPa.
[0058] Comparative Example 1: Preparation method of a starch-based adhesive and its application in wood processing
[0059] Steps (1) to (4) and step (6) are the same as the corresponding steps in Example 1, except for step (5). In step (5) of this comparative example, no curing agent glutaraldehyde is added, and the other parameters are the same.
[0060] The shear strength of the bonded wood board was measured at room temperature to be 7.79±0.79MPa, the shear strength after soaking in room temperature water for 3 hours was 0.70±0.14MPa, and the shear strength after soaking in 60°C hot water for 3 hours was 0.20±0.07MPa. This indicates that the bonded wood board of this comparative example has poor hot water resistance and does not meet the national standard (GB / T 9846-2015) requirement of 0.7MPa.
[0061] Comparative Example 2: Preparation method of a starch-based adhesive and its application in wood processing
[0062] Steps (2) to (6) are the same as the corresponding steps in Example 3, except for step (1). The high-amylose starch used in step (1) of this comparative example has an amylose content of 68%, and the other parameters are the same.
[0063] The shear strength of the bonded wood board was 5.64±1.18MPa at room temperature, 0.92±0.13MPa after soaking in room temperature water for 3 hours, and 0.59±0.07MPa after soaking in 60°C hot water. This indicates that the bonded wood board in this comparative example has poor hot water resistance and does not meet the national standard (GB / T 9846-2015) requirement of 0.7MPa.
[0064] Comparative Example 3: Preparation method of a starch-based adhesive and its application in wood processing
[0065] Steps (2) to (6) are the same as the corresponding steps in Example 3, except for step (1). The high-amylose starch used in step (1) of this comparative example is common starch (amylose content is 27%), and the other parameters are the same.
[0066] The shear strength of the bonded wood board was measured to be 4.69±0.86MPa at room temperature, 1.10±0.18MPa after soaking in room temperature water for 3 hours, and 0.59±0.13MPa after soaking in 60°C hot water. This indicates that the bonded wood board in this comparative example has poor hot water resistance and does not meet the national standard (GB / T 9846-2015) requirement of 0.7MPa.
[0067] Comparative Example 4: Preparation method of a starch-based adhesive and its application in wood processing
[0068] Steps (1), (2), (4), (5) and (6) are the same as the corresponding steps in Example 1, except for step (3). In step (3) of this comparative example, 1 mol / L hydrochloric acid is not added to adjust the pH (at this time, pH=about 8, weak alkalinity).
[0069] The shear strength of the bonded wood board was measured to be 5.53±0.45MPa at room temperature, 0.75±0.24MPa after soaking in room temperature water for 3 hours, and 0.15±0.08MPa after soaking in 60°C hot water for 3 hours. This indicates that the bonded wood board of this comparative example has poor hot water resistance and does not meet the national standard (GB / T 9846-2015) requirement of 0.7MPa.
[0070] Comparative Example 5: Preparation method and application of a starch-based water-resistant flame-retardant adhesive (see invention patent CN115340832A for details)
[0071] The starch adhesive was prepared according to Example 1 of patent CN115340832A, and the specific steps were as follows:
[0072] (1) Weigh 25 g of calcium chloride and add it to 50 mL of water. Stir and dissolve until it becomes clear to obtain a calcium chloride solution.
[0073] (2) Weigh 20 g of high-amylose corn starch (amylose content: 68%), add it to the solution in (1), and stir evenly to form a starch / calcium chloride suspension.
[0074] (3) The suspension in (2) is heated to 75°C for 30 minutes while stirring to obtain a transparent colloidal fluid.
[0075] (4) Weigh 1 g of urea-formaldehyde resin and dissolve it in 0.6 g of water and stir evenly to obtain a colloidal fluid;
[0076] (5) Add the urea-formaldehyde resin glue in (4) to the starch glue in (3), continue stirring at 75° C. for 30 min to completely blend the urea-formaldehyde resin and the glue, and cool to room temperature to obtain a starch-based water-resistant flame-retardant adhesive.
[0077] (6) Weigh 5 g of the starch-based water-resistant flame-retardant adhesive in (5), heat it at 80° C. for 30 min until the adhesive becomes a fluid state, and apply it to the surface of the wooden board.
[0078] (7) Dry the wood board at 75℃ for 20 minutes to ensure it is firmly bonded.
[0079] (8) After the wood boards dried in (7) were immersed in 500 mL of 60°C hot water for 3 h, 3 to 5 of the 10 bonded wood boards had debonded, and the shear strengths of the remaining bonded wood boards were all below 0.1 MPa, which did not meet the national standard (GB / T 9846-2015) requirement of 0.7 MPa.
[0080] It can be seen from Examples 1-3 and Comparative Examples 1-5 that the starch-based adhesive prepared by the method of the present invention and the curing agent not only have strong bonding strength, but also can maintain good bonding strength after being soaked in room temperature water or hot water for a long time ( Figure 1 When applied to wood processing, the adhesive can still provide good bonding strength even after long-term immersion in room temperature water or 60°C hot water, meeting the requirements of the latest national standard (GB / T 17657-2022) and has broad application prospects.
[0081] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. Application of a starch-based adhesive in wood processing, characterized in that: Apply starch-based adhesive evenly on the surface of the wood board, add curing agent, press and dry the wood board, and the wood board can be firmly bonded by starch-based adhesive. Even if it is immersed in room temperature water or 60℃ hot water for a long time, the adhesive can still provide good bonding strength. The preparation method of the starch-based adhesive comprises the following steps: S1, soaking high-amylose starch with low-concentration alkali solution to obtain starch emulsion; S2, adding a low concentration calcium chloride solution to the starch emulsion, adjusting the pH value of the mixed system to below 5.5, and then heating to form a starch paste; S3. Add urea-formaldehyde resin dissolved in water into starch paste, heat and mix evenly to obtain starch-based adhesive.
2. The use according to claim 1, characterized in that: The curing agent is glutaraldehyde, and the amount of the curing agent is not higher than 10% of the mass of the starch-based adhesive.
3. The use according to claim 1, characterized in that: The high-amylose starch refers to natural starch with an amylose content of 50%-60% in starch granules.
4. The use according to claim 1, characterized in that: The low concentration alkali solution in S1 is a NaOH solution with a mass concentration of 0.5-1.5%, and the low concentration calcium chloride solution in S2 is a calcium chloride solution with a mass concentration of 3-5%.
5. The use according to claim 1, characterized in that: The mass ratio of the high-amylose starch to the low-concentration alkali solution in S1 is 1-2:3, and the mass ratio of the low-concentration calcium chloride solution to the starch emulsion in S2 is 0.3-1:
1.
6. The use according to claim 1, characterized in that: In S2, the pH value of the mixed system is adjusted to 5.0-5.
5.
7. The use according to claim 1, characterized in that: The heating temperature in S2 is not less than 95° C., and the heating time is not less than 30 min.
8. The use according to claim 1, characterized in that: The temperature of the heating and mixing step S3 is not less than 95°C.
9. The use according to claim 1, characterized in that: In S3, when dissolved in water, the mass ratio of urea-formaldehyde resin to water is not higher than 1:
1.
10. The use according to claim 1, characterized in that: In S3, the amount of urea-formaldehyde resin used accounts for 10%-30% of the mass of starch paste.
Citation Information
Patent Citations
Preparation method and application of starch-based waterproof flame-retardant adhesive
CN115340832A