Low-viscosity high-toughness high-thermal-conductivity two-component epoxy pouring sealant
The end epoxy nitrile rubber and spherical alumina filler are prepared by reacting end aminonitrile rubber with epoxy resin, which solves the problem of insufficient viscosity and thermal conductivity of epoxy potting, and improves the fluidity of potting and Thermal conductivity enhances the stability and reliability of the device.
Patent Information
- Application Number
- CN202411307503.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-15
AI Technical Summary
The existing epoxy potting glue has too large viscosity and poor fluidity, which is prone to bubbles and pores, and has insufficient thermal conductivity, which cannot meet the heat dissipation needs of electronic components.
The end-epoxy nitrile rubber is used to react with epoxy resin to produce end-epoxy nitrile rubber as toughening agent and with spherical alumina as filler to improve the compatibility and thermal conductivity of the potting glue, reduce viscosity and cracking defects .
It significantly improves the viscosity, fluidity and toughness of the potting adhesive, reduces pores and cracking defects, increases the reliability and stability of the device, and improves the thermal conductivity, with a thermal conductivity up to 2.91W m-1K-1.
Smart Images

Figure BDA0005049695880000121 
Figure BDA0005049695880000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of potting adhesives, and in particular to a two-component epoxy potting adhesive with low viscosity, high toughness and high thermal conductivity. Background Art
[0002] Epoxy resin (commonly known as Epoxyresin) is a linear structure with two or more epoxy groups in the molecule. It is an epoxy oligomer with a low relative molecular mass and is often in liquid or solid state. The latter can soften and melt into liquid state after heating. At first, due to its low relative molecular mass, epoxy resin lacked mechanical properties and was therefore not used. It was not until 1934 that Schlack used amine compounds and epoxy resin to react to produce high molecular polymers, and research on it gradually became popular. The amine compound here is a curing agent, which reacts chemically with epoxy groups under certain temperature (humidity) conditions to generate a three-dimensional network structure, thereby giving epoxy resin the mechanical properties it lacks. On the other hand, the mixture of polyamine (acid) and epoxy resin has good adhesion, which has led to the rapid development of epoxy resin in industry, with increasing production and types, and has been widely used and developed since 1948. While bisphenol A epoxy resins were widely used, new epoxy resins were also developed: alicyclic epoxy resins were sold in 1956, phenolic epoxy resins were developed in 1959, and halogenated epoxy resins, polyolefin epoxy resins, phenolphthalein epoxy resins, and polyaromatic heterocyclic epoxy resins were also introduced around 1960. Until now, the development and application of epoxy resins are still in the ascendant.
[0003] Epoxy potting adhesives on the market have the following problems: (1) They usually require the addition of a large amount of powder, which results in excessive viscosity and poor fluidity. This does not allow sufficient time for vacuum degassing and vacuum potting processes, resulting in a large number of bubbles, pores and other defects in the workpiece after potting. (2) They are usually hard and brittle, which makes them prone to cracking when exposed to extreme weather conditions such as sudden cold or heat or severe external mechanical shocks, resulting in a decrease in their moisture-proof, dust-proof and impact-proof functions, and poor stability and reliability of the potted workpiece. (3) Their thermal conductivity is usually less than 1.0 W m -1 K -1 , cannot meet the heat dissipation requirements of electronic components.
[0004] Toughening by adding nitrile rubber has become the mainstream direction of epoxy potting glue. There are many types of rubber used to toughen epoxy resins, among which nitrile rubber has been studied the most and has the most obvious effect. According to the difference of its active end groups, there are mainly terminal carboxyl (CTBN), terminal hydroxyl (HTLN), terminal amine (ATBN) and random carboxyl nitrile rubber (RCBN). Previous research mainly used mechanical blending methods. For example, patent CN102391813B discloses an epoxy resin conductive adhesive and a preparation method thereof. The epoxy resin conductive adhesive comprises: epoxy resin, toughening agent, latent curing agent, latent accelerator, solvent, conductive filler, wherein resin 3-10%, toughening agent 1-8%, curing agent 5-10%, accelerator 1-5%, solvent 5-10%, conductive filler 60-85%. The invention improves the toughness of the adhesive by adding nitrile rubber toughening agent blending. When rubber is dissolved in resin, a homogeneous solution is formed. During the curing process, the rubber gradually forms rubber particles and is distributed in the resin, forming an "island structure" with the resin. When the material is subjected to stress, it can promote the orientation, stretching, deformation, hollowing of resin molecules and induce cracks, and other energy-consuming effects, thereby improving the ability of the cured product to resist crack propagation and enhancing its toughness.
[0005] However, the compatibility of commercial nitrile rubber with epoxy resin matrix is poor, and it is difficult to disperse evenly in the matrix, resulting in a sharp increase in viscosity when added in small amounts, and the toughening effect is far lower than expected; in addition, since nitrile rubber itself does not contain active groups that can participate in curing, when added in large amounts, it often causes the degree of cross-linking of the cured product to decrease, thus affecting its tensile strength, bonding strength and other mechanical properties. How to improve the toughening effect of nitrile rubber without having a significant negative impact on fluidity, heat resistance, strength, etc. is an urgent problem to be solved in epoxy resin modification research. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a low-viscosity, high-toughness and high-thermal conductivity two-component epoxy potting glue. The terminal epoxy-butadiene nitrile rubber is synthesized by terminal amino nitrile rubber and epoxy resin, and the terminal epoxy-butadiene nitrile rubber is used as a toughening agent. The epoxy-butadiene nitrile rubber has excellent flexibility and good compatibility with the matrix. The potting glue has excellent viscosity, fluidity and toughness, reduces defects such as pores and cracks after potting, and increases the reliability and stability of the device after potting. Spherical alumina with a high spheroidization rate is used as a filler to avoid the problem of increased viscosity caused by the large amount of powder filler added, further improve the fluidity of the potting glue, and at the same time have excellent thermal conductivity.
[0007] In order to solve the above technical problems, the present invention provides a low-viscosity, high-toughness and high-thermal-conductivity two-component epoxy potting adhesive, which comprises the following raw material components by weight:
[0008] Component A: 75-100 parts of the first epoxy resin, 5-15 parts of toughening agent, 700-900 parts of thermal conductive filler, 2.5-3.5 parts of thixotropic agent, 7-9 parts of coupling agent, 1.5-2.5 parts of defoaming agent, 0.1-0.5 parts of colorant;
[0009] Component B: 80-115 parts of curing agent, 0.25-0.35 parts of accelerator, 700-900 parts of thermal conductive filler, 2.5-3.5 parts of thixotropic agent, 7-9 parts of coupling agent, 1.5-2.5 parts of defoaming agent;
[0010] The toughening agent is an epoxy-terminated nitrile rubber, and the epoxy-terminated nitrile rubber is prepared by reacting amino-terminated nitrile rubber with epoxy resin.
[0011] The present invention firstly reacts amino-terminated nitrile rubber with epoxy resin to synthesize epoxy-terminated nitrile rubber, and then uses the epoxy-terminated nitrile rubber as a toughening agent and blends it with various components of a potting compound. Compared with the existing nitrile rubber, the synthesized epoxy-terminated nitrile rubber has excellent compatibility with a matrix, so that the potting compound has moderate viscosity and excellent fluidity, is suitable for potting of workpieces with large sizes and complex internal structures, and greatly reduces defects such as pores and voids remaining inside the workpiece. In addition, the synthesized epoxy-terminated nitrile rubber has excellent flexibility and toughness, and at the same time, due to its good compatibility with the matrix, it can be evenly dispersed in the matrix, so that its toughening effect is more significant, which can significantly reduce the degree of cracking after potting, and make the potted components have excellent reliability and stability.
[0012] Furthermore, the preparation method of the epoxy-terminated nitrile rubber is as follows: a molar ratio of 1: (2 to 2.4) is mixed with an amino-terminated nitrile rubber and a second epoxy resin, and the mixture is reacted at room temperature for 24 to 36 hours, and excess epoxy compounds are removed by distillation to obtain the epoxy-terminated nitrile rubber. The epoxy-terminated nitrile rubber is synthesized by reacting the amino-terminated nitrile rubber with the epoxy resin. The synthesis method is simple and mild. The prepared epoxy-terminated nitrile rubber has better flexibility than the nitrile rubber on the market and has better compatibility with the matrix.
[0013] Furthermore, the second epoxy resin is 1,4-butanediol diglycidyl ether and / or 1,6-hexanediol diglycidyl ether.
[0014] Furthermore, the thermally conductive fillers of the components A and B are independently selected from one or more of spherical alumina, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide, graphene, carbon nanotubes, carbon fiber powder, aluminum hydroxide and magnesium hydroxide, and the preferred thermally conductive filler is spherical alumina. Spherical alumina is used in combination with synthetic end-epoxy nitrile rubber. Alumina with a high spheroidization rate can be added in large quantities without causing a sharp increase in viscosity. The synthetic end-epoxy nitrile rubber has good compatibility with the matrix and will not cause a significant increase in viscosity. The combination of the two can significantly increase the amount of thermally conductive powder added to the potting glue of the present invention, which makes the potting glue have excellent thermal conductivity, and the thermal conductivity coefficient can reach up to 2.91Wm -1 K -1 .
[0015] Furthermore, the first epoxy resin is one or more of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, and alicyclic epoxy resin; preferably one or more of DER331, DER354, YL-980, jER-1750, and NPEF-170.
[0016] Furthermore, the coupling agents of the components A and B are independently selected from one or more of γ-glycidyloxypropyltrimethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, vinyl tri-tert-butyl peroxide silane, 3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-thiolpropyltriethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, and vinyl tri-tert-butyl peroxide silane.
[0017] Furthermore, the thixotropic agents of the components A and B are independently selected from one or more of modified castor oil, organic bentonite, polyamide wax, and fumed silica.
[0018] Furthermore, the curing agent is one or more of aliphatic amines, modified aliphatic amines, modified alicyclic amines, modified aromatic amines, and phenolic amines; preferably 70. 75-1, One or more of 3227, JH-5473, and XH-419.
[0019] Furthermore, the accelerator is one or more of 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, 2-methylimidazole, 2-phenylimidazole, and 2-ethyl-4-methylimidazole.
[0020] Furthermore, the defoamers of the components A and B are independently selected from one or more of silicone defoamers, polyether defoamers, and mineral oil defoamers.
[0021] Furthermore, the colorant is an organic dye and / or an inorganic dye, such as one or more of yellow iron oxide, red iron oxide, and carbon black, including but not limited to these.
[0022] Beneficial effects of the present invention:
[0023] The present invention reacts amino-terminated nitrile rubber with epoxy resin to synthesize epoxy-terminated nitrile rubber, which is then used as a toughening agent and blended with various components of a potting compound. Compared with the existing nitrile rubber, the synthesized epoxy-terminated nitrile rubber has excellent compatibility with a matrix, so that the potting compound has moderate viscosity and excellent fluidity, is suitable for potting of workpieces with large sizes and complex internal structures, and greatly reduces defects such as residual pores and voids inside the workpiece.
[0024] The epoxy-terminated nitrile rubber synthesized by the present invention has excellent flexibility and can be evenly dispersed in the matrix due to its good compatibility with the matrix, so that its toughening effect is more significant, which can significantly reduce the degree of cracking after potting, so that the components after potting have excellent reliability and stability.
[0025] The present invention uses spherical alumina and synthetic terminal epoxy-butadiene nitrile rubber in combination to achieve synergistic effects. Alumina with a high spheroidization rate can be added in large quantities without causing a sharp increase in viscosity. The synthetic terminal epoxy-butadiene nitrile rubber has good compatibility with the matrix and will not cause a significant increase in viscosity. The combination of the two can significantly increase the amount of thermal conductive powder added to the potting glue, which enables the potting glue to have excellent thermal conductivity, and the thermal conductivity coefficient can reach up to 2.91 W m -1 K -1 . DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0027] Example 1
[0028] This embodiment relates to a low-viscosity, high-toughness, and high-thermal-conductivity two-component epoxy potting adhesive, which includes the following raw material components by weight:
[0029] Component A: 90 parts of epoxy resin jER-1750, 10 parts of toughening agent, 800 parts of thermal conductive filler spherical alumina, 3 parts of thixotropic agent fumed silica, 8 parts of coupling agent γ-glycidyloxypropyl trimethoxysilane, 2 parts of silicone defoamer BYK-070, 0.3 parts of colorant carbon black;
[0030] Component B: 35 parts of curing agent 75-1, 65 parts of curing agent 3227, 0.3 parts of accelerator 2,4,6-tris(dimethylaminomethyl)phenol, 800 parts of thermal conductive filler spherical alumina, 3 parts of thixotropic agent fumed silica, 8 parts of coupling agent γ-aminopropyltriethoxysilane, 2 parts of defoaming agent BYK-088;
[0031] Among them, the toughening agent is epoxy-terminated nitrile rubber, and its preparation method is as follows: add 42.42g of 1,4-butanediol diglycidyl ether into a thoroughly dried sealed reactor, add 315g of amino-terminated nitrile rubber (liquid nitrile rubber, molecular weight between 3000 and 4000, from Huntsman, USA) dropwise at room temperature under stirring, stir the reaction at room temperature for 24 hours, and then distill to remove excess epoxy compounds to obtain epoxy-terminated nitrile rubber.
[0032] In this embodiment, the preparation method of component A is as follows: adding the epoxy resin, toughening agent, thermal conductive filler, thixotropic agent, coupling agent, defoaming agent and colorant in the above proportion to a stirring kettle, stirring until completely dispersed and uniform; then placing the stirred glue in a planetary homogenizer for mixing and degassing, and after degassing, component A can be obtained. The preparation method of component B is as follows: adding the curing agent, accelerator, thermal conductive filler, thixotropic agent, coupling agent and defoaming agent in the above proportion to a stirring kettle, stirring until completely dispersed and uniform; then placing the stirred glue in a planetary homogenizer for mixing and degassing, and after degassing, component B can be obtained.
[0033] Example 2
[0034] The difference between this embodiment and embodiment 1 is that it includes the following raw material components:
[0035] Component A: 75 parts of epoxy resin jER-1750, 5 parts of toughening agent, 700 parts of thermal conductive filler spherical alumina, 2.5 parts of thixotropic agent fumed silica, 7.0 parts of coupling agent γ-glycidyloxypropyl trimethoxysilane, 1.5 parts of silicone defoamer BYK-070, 0.25 parts of colorant carbon black;
[0036] Component B: 30 parts of curing agent 75-1, 50 parts of curing agent 3227, 0.25 parts of promoter 2,4,6-tris(dimethylaminomethyl)phenol, 700 parts of thermal conductive filler spherical alumina, 2.5 parts of thixotropic agent fumed silica, 7 parts of coupling agent γ-aminopropyltriethoxysilane, and 1.5 parts of defoaming agent BYK-088.
[0037] The other steps remain unchanged.
[0038] Example 3
[0039] The difference between this embodiment and embodiment 1 is that it includes the following raw material components:
[0040] Component A: 100 parts of epoxy resin jER-1750, 15 parts of toughening agent, 900 parts of thermal conductive filler spherical alumina, 3.5 parts of thixotropic agent fumed silica, 9.0 parts of coupling agent γ-glycidyloxypropyl trimethoxysilane, 2.5 parts of silicone defoamer BYK-070, 0.35 parts of colorant carbon black;
[0041] Component B: 40 parts of curing agent 75-1, 75 parts of curing agent 3227, 0.35 parts of promoter 2,4,6-tris(dimethylaminomethyl)phenol, 900 parts of thermal conductive filler spherical alumina, 3.5 parts of thixotropic agent fumed silica, 9.0 parts of coupling agent γ-aminopropyltriethoxysilane, and 2.5 parts of defoaming agent BYK-088.
[0042] The other steps remain unchanged.
[0043] Example 4
[0044] The difference between this embodiment and embodiment 1 is that it includes the following raw material components:
[0045] Component A: 84.4 parts of epoxy resin jER-1750, 8.4 parts of toughening agent, 750 parts of thermal conductive filler spherical alumina, 2.8 parts of thixotropic agent fumed silica, 7.5 parts of coupling agent γ-glycidyloxypropyl trimethoxysilane, 1.9 parts of silicone defoamer BYK-070, 0.28 parts of colorant carbon black;
[0046] Component B: 32.8 parts of curing agent 75-1, 60.9 parts of curing agent 3227, 0.28 parts of promoter 2,4,6-tris(dimethylaminomethyl)phenol, 750 parts of thermal conductive filler spherical alumina, 2.8 parts of thixotropic agent fumed silica, 7.5 parts of coupling agent γ-aminopropyltriethoxysilane, and 1.9 parts of defoaming agent BYK-088.
[0047] The other steps remain unchanged.
[0048] Example 5
[0049] The difference between this embodiment and embodiment 1 is that it includes the following raw material components:
[0050] Component A: 95.6 parts of epoxy resin jER-1750, 12.6 parts of toughening agent, 850 parts of thermal conductive filler spherical alumina, 3.2 parts of thixotropic agent fumed silica, 8.5 parts of coupling agent γ-glycidyloxypropyl trimethoxysilane, 2.1 parts of silicone defoamer BYK-070, 0.32 parts of colorant carbon black;
[0051] Component B: 37.2 parts of curing agent 75-1, 69.1 parts of curing agent 3227, 0.32 parts of promoter 2,4,6-tris(dimethylaminomethyl)phenol, 850 parts of thermal conductive filler spherical alumina, 3.2 parts of thixotropic agent fumed silica, 8.5 parts of coupling agent γ-aminopropyltriethoxysilane, and 2.1 parts of defoaming agent BYK-088.
[0052] The other steps remain unchanged.
[0053] Example 6
[0054] The difference between this embodiment and embodiment 1 is that the preparation method of the toughening agent-terminated epoxy-based nitrile rubber is as follows:
[0055] Add 48.36 g of 1,6-hexanediol diglycidyl ether into a thoroughly dried sealed reactor, and add 315 g of amino-terminated nitrile rubber dropwise at room temperature under stirring. Stir the reaction at room temperature for 36 hours, then distill off the excess epoxy compound to obtain epoxy-terminated nitrile rubber.
[0056] The other steps remain unchanged.
[0057] Example 7
[0058] The difference between this embodiment and embodiment 6 is that the following raw material components are included:
[0059] Component A: 75 parts of epoxy resin jER-1750, 5 parts of toughening agent, 700 parts of thermal conductive filler spherical alumina, 2.5 parts of thixotropic agent fumed silica, 7.0 parts of coupling agent γ-glycidyloxypropyl trimethoxysilane, 1.5 parts of silicone defoamer BYK-070, 0.25 parts of colorant carbon black;
[0060] Component B: 30 parts of curing agent 75-1, 50 parts of curing agent 3227, 0.25 parts of promoter 2,4,6-tris(dimethylaminomethyl)phenol, 700 parts of thermal conductive filler spherical alumina, 2.5 parts of thixotropic agent fumed silica, 7 parts of coupling agent γ-aminopropyltriethoxysilane, and 1.5 parts of defoaming agent BYK-088.
[0061] The other steps remain unchanged.
[0062] Example 8
[0063] The difference between this embodiment and embodiment 6 is that the following raw material components are included:
[0064] Component A: 100 parts of epoxy resin jER-1750, 15 parts of toughening agent, 900 parts of thermal conductive filler spherical alumina, 3.5 parts of thixotropic agent fumed silica, 9.0 parts of coupling agent γ-glycidyloxypropyl trimethoxysilane, 2.5 parts of silicone defoamer BYK-070, 0.35 parts of colorant carbon black;
[0065] Component B: 40 parts of curing agent 75-1, 75 parts of curing agent 3227, 0.35 parts of promoter 2,4,6-tris(dimethylaminomethyl)phenol, 900 parts of thermal conductive filler spherical alumina, 3.5 parts of thixotropic agent fumed silica, 9.0 parts of coupling agent γ-aminopropyltriethoxysilane, and 2.5 parts of defoaming agent BYK-088.
[0066] The other steps remain unchanged.
[0067] Example 9
[0068] The difference between this embodiment and embodiment 6 is that the following raw material components are included:
[0069] Component A: 84.4 parts of epoxy resin jER-1750, 8.4 parts of toughening agent, 750 parts of thermal conductive filler spherical alumina, 2.8 parts of thixotropic agent fumed silica, 7.5 parts of coupling agent γ-glycidyloxypropyl trimethoxysilane, 1.9 parts of silicone defoamer BYK-070, 0.28 parts of colorant carbon black;
[0070] Component B: 32.8 parts of curing agent 75-1, 60.9 parts of curing agent 3227, 0.28 parts of promoter 2,4,6-tris(dimethylaminomethyl)phenol, 750 parts of thermal conductive filler spherical alumina, 2.8 parts of thixotropic agent fumed silica, 7.5 parts of coupling agent γ-aminopropyltriethoxysilane, and 1.9 parts of defoaming agent BYK-088.
[0071] The other steps remain unchanged.
[0072] Example 10
[0073] The difference between this embodiment and embodiment 6 is that the following raw material components are included:
[0074] Component A: 95.6 parts of epoxy resin jER-1750, 12.6 parts of toughening agent, 850 parts of thermal conductive filler spherical alumina, 3.2 parts of thixotropic agent fumed silica, 8.5 parts of coupling agent γ-glycidyloxypropyl trimethoxysilane, 2.1 parts of silicone defoamer BYK-070, 0.32 parts of colorant carbon black;
[0075] Component B: 37.2 parts of curing agent 75-1, 69.1 parts of curing agent 3227, 0.32 parts of promoter 2,4,6-tris(dimethylaminomethyl)phenol, 850 parts of thermal conductive filler spherical alumina, 3.2 parts of thixotropic agent fumed silica, 8.5 parts of coupling agent γ-aminopropyltriethoxysilane, and 2.1 parts of defoaming agent BYK-088.
[0076] The other steps remain unchanged.
[0077] Embodiment 11
[0078] The difference between this embodiment and embodiment 6 is that the amount of spherical alumina as a thermally conductive filler added to components A and B is 900 parts.
[0079] The other steps remain unchanged.
[0080] Comparative Example 1
[0081] The difference between this comparative example and Example 2 is that the amount of toughening agent added is 4.0 parts, and the other steps remain unchanged.
[0082] Comparative Example 2
[0083] The difference between this comparative example and Example 3 is that the amount of toughening agent added is 16 parts, and the other steps remain unchanged.
[0084] Comparative Example 3
[0085] The difference between this comparative example and Example 7 is that the amount of toughening agent added is 4.0 parts, and the other steps remain unchanged.
[0086] Comparative Example 4
[0087] The difference between this comparative example and Example 8 is that the amount of toughening agent added is 16 parts, and the other steps remain unchanged.
[0088] Comparative Example 5
[0089] The difference between this comparative example and Example 1 is that the toughening agent is commercially available nitrile rubber, and the other steps remain unchanged.
[0090] Comparative Example 6
[0091] The difference between this comparative example and Example 1 is that no toughening agent is added, and other steps remain unchanged.
[0092] Test Case
[0093] The performance tests of the potting glues of the embodiments and comparative examples are as follows:
[0094] A. Viscosity
[0095] (1) Preparation of viscosity test samples
[0096] Mix component A and component B in a mass ratio of 1:1, and then pour the mixed sample along the inner wall of the sample cup to reduce the bubbles inside the sample. The sample volume should be between 3 and 5 mL, and the sample should not overflow after the rotor is immersed.
[0097] (2) Testing process
[0098] The sample is placed in the instrument and kept at 25°C for 30 minutes before the test begins. The test process is carried out in accordance with the standard GB / T2794-2013. The test instrument is a Brookfield viscometer, model HBDV-Ⅱ+P, and the rotor is a 14# rotor.
[0099] B. Extrusion rate
[0100] The prepared A and B components were divided into 50mL two-component rubber tubes, and placed vertically at room temperature with the rubber outlet facing downward for 7 days before testing. During the test, the rubber liquid was squeezed out through the mixing tube, and the mass of the rubber liquid squeezed out within 1 minute was weighed on a balance. The thrust used during extrusion was fixed at about 300N.
[0101] C. Impact strength
[0102] (1) Preparation of impact strength test samples
[0103] Mix component A and component B in a mass ratio of 1:1, then pour the mixed glue into the mold and cure it at room temperature for 24 hours to obtain the test sample. Sample requirements: length 80mm, width 10mm, thickness 4mm, and no cracks or bubbles on the surface.
[0104] (2) Testing process
[0105] The sample is placed horizontally on the fixture, and the fixture needs to clamp the sample to ensure that it does not move when impacted. The test process is carried out in accordance with the standard GB / T 1043.1-2008. The equipment used is the liquid crystal plastic pendulum impact tester of Shenzhen Wance Testing Equipment Co., Ltd., model PIT501B-2.
[0106] D. Thermal conductivity
[0107] (1) Preparation of thermal conductivity test samples
[0108] Mix component A and component B in a mass ratio of 1:1, then pour the mixed glue into the mold and cure it at room temperature for 24 hours to obtain the test sample. Sample requirements: diameter 30mm, thickness ≤5mm, and smooth surface.
[0109] (2) Testing process
[0110] Coat a layer of thermal conductive silicone grease on the surface of the prepared sample, then put it into the equipment to start the test. The test process is carried out according to the standard ASTM D5470. The equipment used for the test is Xiangtan Instrument DRL-V thermal conductivity tester, with a cold pole temperature of 30℃, a hot pole temperature of 70℃, and a test pressure of 200N.
[0111] The test results of the potting glue obtained in the embodiment and the comparative example are shown in Table 1:
[0112] Table 1
[0113]
[0114]
[0115] Referring to Table 1, it can be seen from the comparison between Example 1 and Comparative Example 5 that after the toughening agent is replaced with commercially available nitrile rubber, due to its poor compatibility with the matrix and poor flexibility, the viscosity after mixing is too high, reaching 288000cPs, the extrusion speed is reduced to 15g / min, the fluidity is poor, and it is easy to cause defects such as residual pores and voids in the potted workpiece, thereby causing the decrease of its impact strength and thermal conductivity, which are reduced to 11kJ / m 2 and 2.33Wm -1 K -1 From the comparison between Example 1 and Comparative Example 6, it can be seen that when no toughening agent is added, the commercially available nitrile rubber as a toughening agent has a similar effect as that of Comparative Example 5, with a high viscosity after mixing and a low extrusion rate, resulting in a final impact strength as low as 8 kJ / m 2 .
[0116] From the comparison between Example 2 and Comparative Example 1, Example 3 and Comparative Example 2, Example 7 and Comparative Example 3, and Example 8 and Comparative Example 4, it can be seen that when the ratio of the toughening agent-terminated epoxy nitrile rubber exceeds the specified range of the present invention, the corresponding viscosity after mixing is significantly increased, especially the viscosity after mixing of Comparative Example 3 is as high as 253000 cPs, the corresponding extrusion speed is reduced to 19 g / min, the fluidity is reduced, and defects such as pores and voids are easily left in the potted workpiece, which leads to a decrease in the impact strength and thermal conductivity of the workpiece after potting.
[0117] From the comparison between Example 6 and Example 11, it can be seen that the increase in the amount of spherical alumina added will lead to an increase in the viscosity after mixing, which in turn leads to a decrease in the extrusion rate and impact strength, but the thermal conductivity is improved to as high as 2.91 W m -1 K -1. Therefore, it is necessary to adjust the addition amount of the epoxy-terminated nitrile rubber and the spherical alumina so that the two can work together to obtain excellent viscosity, extrusion rate, impact strength and thermal conductivity after mixing to meet practical applications. It can be seen from Examples 1-5 and Examples 6-11 that the potting compound prepared within the ratio range defined by the present invention has excellent viscosity and fluidity, thereby obtaining a potting part with high impact strength and excellent thermal conductivity.
[0118] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A low-viscosity, high-toughness and high-thermal-conductivity two-component epoxy potting adhesive, characterized in that: By weight, it includes the following raw material components: Component A: 75-100 parts of the first epoxy resin, 5-15 parts of toughening agent, 700-900 parts of thermal conductive filler, 2.5-3.5 parts of thixotropic agent, 7-9 parts of coupling agent, 1.5-2.5 parts of defoaming agent, 0.1-0.5 parts of colorant; Component B: 80-115 parts of curing agent, 0.25-0.35 parts of accelerator, 700-900 parts of thermal conductive filler, 2.5-3.5 parts of thixotropic agent, 7-9 parts of coupling agent, 1.5-2.5 parts of defoaming agent; Wherein, the toughening agent is an epoxy-terminated nitrile rubber, and the epoxy-terminated nitrile rubber is prepared by reacting amino-terminated nitrile rubber with epoxy resin.
2. The low-viscosity, high-toughness, high-thermal-conductivity two-component epoxy potting adhesive according to claim 1, characterized in that: The preparation method of the epoxy-terminated nitrile rubber is as follows: amino-terminated nitrile rubber and a second epoxy resin are mixed in a molar ratio of 1: (2-2.4), reacted at room temperature for 24-36 hours, and distilled to remove excess epoxy compounds to obtain the epoxy-terminated nitrile rubber.
3. The low-viscosity, high-toughness, high-thermal-conductivity two-component epoxy potting adhesive according to claim 2, characterized in that: The second epoxy resin is 1,4-butanediol diglycidyl ether and / or 1,6-hexanediol diglycidyl ether.
4. The low-viscosity, high-toughness, high-thermal-conductivity two-component epoxy potting adhesive according to claim 1, characterized in that: The thermally conductive fillers of the components A and B are independently selected from one or more of spherical aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide, graphene, carbon nanotubes, carbon fiber powder, aluminum hydroxide and magnesium hydroxide.
5. The low-viscosity, high-toughness, high-thermal-conductivity two-component epoxy potting adhesive according to claim 1, characterized in that: The first epoxy resin is one or more of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, and alicyclic epoxy resin.
6. The low-viscosity, high-toughness, high-thermal-conductivity two-component epoxy potting adhesive according to claim 1, characterized in that: The coupling agents of component A and component B are independently selected from one or more of γ-glycidyloxypropyltrimethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, vinyl tri-tert-butyl peroxide silane, 3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-thiolpropyltriethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, and vinyl tri-tert-butyl peroxide silane.
7. The low-viscosity, high-toughness, high-thermal-conductivity two-component epoxy potting adhesive according to claim 1, characterized in that: The thixotropic agents of the components A and B are independently selected from one or more of modified castor oil, organic bentonite, polyamide wax, and fumed silica.
8. The low-viscosity, high-toughness, high-thermal-conductivity two-component epoxy potting adhesive according to claim 1, characterized in that: The curing agent is one or more of aliphatic amine, modified aliphatic amine, modified alicyclic amine, modified aromatic amine and phenolic amine.
9. The low-viscosity, high-toughness, high-thermal-conductivity two-component epoxy potting adhesive according to claim 1, characterized in that: The accelerator is one or more of 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, 2-methylimidazole, 2-phenylimidazole, and 2-ethyl-4-methylimidazole.
10. The low-viscosity, high-toughness, high-thermal-conductivity two-component epoxy potting adhesive according to claim 1, characterized in that: The defoamers of component A and component B are independently selected from one or more of silicone defoamers, polyether defoamers, and mineral oil defoamers.
Citation Information
Patent Citations
Single-component epoxy resin conductive adhesive
CN102391813B
Cited By
An environmentally friendly toughened epoxy potting compound, adhesive and composite toughening agent
CN123042646A