High-speed steel electric furnace smelting process
By adjusting the order of raw material addition and adding oxygen blowing steps, the reduction slag production and refining steps are integrated, which solves the problems of long smelting cycle and low liquid cleanliness in high-speed steel electric furnace smelting, achieving a more efficient smelting process and a lower Production cost.
Patent Information
- Application Number
- CN202411011281.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing high-speed steel electric furnace smelting process, the smelting cycle is relatively long, the smelting efficiency is low, and the reduction slag production and refining function overlap, resulting in low cleanliness of the steel and increasing inclusions.
Adjust the order of adding raw materials, add an oxygen blowing step, integrate the reduction slag with the refining step, avoid feeding aluminum after refining, shorten the smelting cycle, improve the utilization rate of precious metals, and reduce inclusions.
The smelting cycle is shortened, the raw material utilization rate is improved, the number and size of inclusions in the molten steel is reduced, the cleanliness of the molten steel and the alloy composition control accuracy are improved, and the production cost is reduced.
Smart Images

Figure CN118957199A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a high-speed steel electric furnace smelting process. Background Art
[0002] High-speed steel is the main material for manufacturing tools with complex shapes and difficult grinding. High-speed steel has a high carbon content and requires the addition of a variety of alloying elements such as tungsten, molybdenum, chromium and vanadium during its preparation, which allows it to maintain high hardness and good wear resistance even at high temperatures.
[0003] The existing high-speed steel smelting mostly adopts electric arc furnace smelting, which has high thermal efficiency, easy to control the temperature of molten steel and high smelting quality. The general process of smelting high-speed steel in electric arc furnace includes electric furnace smelting, LF refining, VD refining and die casting. The main functions of electric furnace smelting and LF refining are to melt the raw materials at high temperature and remove impurities to provide the purity of molten steel.
[0004] The specific steps of electric furnace smelting and LF refining in the prior art are as follows: the raw materials are loaded into the electric furnace in advance before power is turned on, and then the power is turned on to melt. After 60 minutes of smelting, the secondary feeding is carried out and the smelting is continued. After 90 minutes of smelting, oxygen blowing is started to assist melting, and ferrosilicon powder is added to the furnace during the oxygen blowing process. After continuing to smelt for about 20 minutes, oxygen blowing is stopped, and calcium carbide, carbon powder and ferrosilicon powder are added to the furnace to pre-reduce the slag system, and then the slag is removed. After the slag removal is completed, calcium carbide, lime and other reducing slag are continued to be added to the furnace, and finally aluminum is fed to tap the steel. After tapping the steel, the ladle is moved to the refining position for refining. During the refining, lime and ferrosilicon powder are added to the refining furnace to adjust the slag system. After the slag is made, alloy is added to it according to the test results. Finally, the power is turned off and the refining is completed by blowing lightly for 5 minutes.
[0005] The above-mentioned electric furnace smelting and LF refining have the following problems: 1. The electric furnace smelting cycle is relatively long, with a single furnace cycle of about 165 minutes, and the smelting efficiency is low; 2. The reduction period function in electric furnace smelting overlaps with the function of LF refining, and the smelting process design is unreasonable; 3. After the completion of LF refining, the amount of alumina and magnesium-aluminum oxide in the inclusions in the molten steel increases greatly, and the cleanliness of the molten steel is low. Summary of the invention
[0006] In view of the above-mentioned problems existing in the current high-speed steel smelting process, the present invention provides a high-speed steel electric furnace smelting process, which greatly shortens the smelting market, improves the utilization rate of precious metals in the raw materials, and reduces the number and size of inclusions in the molten steel by adjusting the order of adding raw materials, adding an oxygen blowing and fluxing step, integrating the reducing slag making and refining steps, and avoiding feeding aluminum after the refining is completed. The specific technical scheme is as follows:
[0007] First, the present invention provides a high speed steel electric furnace smelting process, comprising the following steps:
[0008] S1 Raw material melting: add primary material to the electric furnace and then turn on the power for smelting. Perform oxygen blowing to assist melting during smelting. After molten steel appears, add secondary material to the electric furnace to continue smelting and perform secondary oxygen blowing to assist melting. Add ferrosilicon powder during oxygen blowing. Adjust the power of the electric furnace and continue smelting until the secondary oxygen blowing to assist melting stops.
[0009] S2 Pre-reduction, steel tapping and reducing slag making: Add reducing agent I and alloy into the furnace to pre-reduce the smelting slag system, and perform slag removal after the pre-reduction. After the slag removal, add aluminum to tap the steel, and add reducing agent II into the ladle to make reducing slag during the tapping process;
[0010] S3 refining: After slag making, the molten steel is transferred to the LF refining area for electric refining and slag-forming agent is added to adjust the refined slag system. According to the composition of the refined slag system, alloys are added to continue refining. After refining, it is gently blown and then the next process is carried out.
[0011] Furthermore, the primary material in step S1 includes scrap steel, raw iron, high tungsten, tungsten-iron alloy, and molybdenum-iron alloy; the secondary material includes returned iron filings and 6524 steel.
[0012] Furthermore, in step S1, after the primary material is smelted by electricity for 40 to 45 minutes, oxygen blowing is performed for a first time, and the time of the first oxygen blowing is 15 to 17 minutes; after the primary material is smelted by electricity for 60 to 65 minutes, the secondary material is added, and after the secondary material is smelted for 10 to 12 minutes, oxygen blowing is performed for a second time, and the time of the second oxygen blowing is 15 to 17 minutes.
[0013] Furthermore, in step S1, the reducing agent I includes fluorite and calcium carbide, the alloy includes tungsten-iron alloy and molybdenum-iron alloy; and the pre-reduction reaction time is 10 to 15 minutes.
[0014] Furthermore, in step S2, the adding of aluminum is adding aluminum wire, and the speed of adding the aluminum wire is 4-5 m / s.
[0015] Furthermore, in step S2, the reducing agent II includes lime, calcium carbide and ferrosilicon powder, and the lime is added into the steel bag in advance.
[0016] Furthermore, the refined slag system in step S3 needs to meet the following indicators: basicity range 3-5; Si0 2 Content is 10-18%; A1203 content is 25-35%; MgO content is 5-7%; (FeO+Mn0) content is less than 1%.
[0017] Furthermore, the alloy added in step S3 includes one or more of vanadium-iron alloy, manganese-iron alloy and chromium-containing alloy; the alloys are added in sequence at intervals of 10 minutes.
[0018] Furthermore, the blowing time in step S3 is 5 to 10 minutes.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1) In view of the problem of the long smelting cycle of existing high-speed steel electric furnaces, the present invention studies and adjusts the electric furnace smelting and refining process, adds an oxygen blowing step before the secondary feeding, increases the melting rate of the raw materials by blowing oxygen, and shortens the melting period of the raw materials. At the same time, the inventors found that the reducing slag making stage in the existing electric furnace smelting process overlaps with the function of the refining furnace, which results in the failure to fully utilize the capacity of the refining furnace and prolongs the electric furnace smelting cycle. Therefore, in the present invention, the reducing slag making is moved to the steel-out and aluminum-adding step, and this function is transferred to the refining process. In this way, the refining function of the refining furnace is utilized without increasing the original refining time, further shortening the entire smelting cycle, and the entire smelting process can be completed within 170 minutes.
[0021] 2) The present invention adjusts the order of adding ingredients in the existing smelting process, and adds 6524 steel containing V and Cr and returned iron filings into the secondary material, thereby avoiding the loss of V and Cr due to oxidation during the oxygen blowing process, improving the recovery rate of precious metal elements, facilitating the control of the content of alloy components, and reducing production costs.
[0022] 3) In the prior art, aluminum will continue to be fed after refining to remove oxygen from the steel and reduce oxide inclusions, thereby improving the purity and quality of the steel and enhancing the mechanical properties and wear resistance of the steel. However, since aluminum feeding after refining will produce some aluminum oxide inclusions, despite the presence of light blowing, the newly generated aluminum oxide inclusions do not have sufficient time to float up, resulting in the appearance of large-sized inclusions. In response to this problem, the present invention adds all the required aluminum materials at the time of steel tapping, so that the deoxidation and grain refinement effects of aluminum can be fully utilized during subsequent refining without additionally producing large-sized inclusion oxides, thereby improving the purity of the smelting. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic diagram of a high-speed steel electric furnace smelting process according to an embodiment of the present invention;
[0024] Figure 2 It is a schematic flow diagram of the smelting process in Comparative Example 1 of the present invention;
[0025] Figure 3 ASPEX automatic scanning electron microscope image (right) and size statistical result image (left) of the steel sample in the embodiment of the present invention;
[0026] Figure 4 The ASPEX automatic scanning electron microscope image (right) and the size statistical result image (left) of the steel sample in Comparative Example 3 of the present invention are shown. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present invention more clear, the technical solution of the present invention will be clearly and completely described below in conjunction with embodiments.
[0028] Example
[0029] This embodiment provides a high speed steel electric furnace smelting process, comprising the following steps:
[0030] S1 Raw material melting: add primary material to the electric furnace and then turn on the power for smelting. Perform oxygen blowing to assist melting during smelting. After molten steel appears, add secondary material to the electric furnace to continue smelting and perform secondary oxygen blowing to assist melting. Add ferrosilicon powder during oxygen blowing. Adjust the power of the electric furnace and continue smelting until the secondary oxygen blowing to assist melting stops.
[0031] Specifically, the primary material is added to the electric furnace. This embodiment takes the production of a 20t electric furnace as an example. The primary material includes 6700kg of scrap steel, 870kg of tungsten iron alloy, 820kg of molybdenum iron alloy, 1000kg of raw iron and 750kg of high tungsten. Turn on the electric furnace and adjust the voltage value of the electric furnace to 260V and the current value to 20kV. After smelting for 40min, oxygen blowing is performed for fluxing, the oxygen blowing time is 15min, and the oxygen blowing pressure is 0.8MPa. After continuing to smelt for 20 to 35min, the secondary material is added to the electric furnace for smelting. The secondary material includes 5200kg of returned iron scraps and 5000kg of 6524 steel. After smelting for 15min, secondary oxygen blowing is performed for fluxing, and ferrosilicon powder is added to the furnace at the same time, and the voltage of the electric furnace is adjusted to 225V and the current to 15kV. After continuing to smelt for 10 to 15min, the voltage of the electric furnace is adjusted to 210V, and the oxygen blowing is stopped after the current stabilizes to 13kV.
[0032] S2 Pre-reduction, steel tapping and reducing slag making: Add reducing agent I and alloy into the furnace to pre-reduce the smelting slag system, and perform slag removal after the pre-reduction. After the slag removal, add aluminum to tap the steel, and add reducing agent II into the ladle to make reducing slag during the tapping process;
[0033] Specifically, after stopping oxygen blowing and fluxing, fluorite, calcium carbide, tungsten-iron alloy and molybdenum-iron alloy are added into the furnace to perform a pre-reduction reaction on the smelting slag system, and the slag is removed after the reaction for 10 to 15 minutes. After the electric furnace is removed, aluminum is added to tap the steel. In this embodiment, aluminum wire is added to the molten steel at a speed of 4 m / s. After adding aluminum, lime is added to the ladle in advance, and calcium carbide and ferrosilicon powder are added to the ladle during the tapping process to make reducing slag.
[0034] S3 refining: After slag making, the molten steel is transferred to the LF refining area for electric refining and slag-forming agent is added to adjust the refined slag system. According to the composition of the refined slag system, alloys are added to continue refining. After refining, it is gently blown and then the next process is carried out.
[0035] Specifically, after slag making is completed, the molten steel is transferred to the LF refining furnace, and the refining furnace voltage is set to 260V and the current is set to 20kV. After stabilization, lime, calcium carbide and ferrosilicon powder are added to the refining furnace to adjust the refining slag system. After the refining slag system is adjusted, samples are taken for testing. According to the test results of the sampled components, vanadium-ferroalloy, manganese-ferroalloy and chromium-containing alloy can be added to the refining furnace for further refining. In this embodiment, the refining slag system needs to meet the basicity range of 3 to 5; SiO 2 Content 10~18%;Al 2 O 3 The technical indicators are as follows: content 25-35%; Mg0 content 5-7%; (Fe0+Mn0) content less than 1%. The alloy components are added in batches, and the next alloy is added after the alloy is refined for 10 minutes. After the refining is completed, the power is turned off and the light blowing is performed for 5 minutes. After the light blowing is completed, proceed to the next step.
[0036] By installing the implementation method of this embodiment, the total duration of the S1 raw material melting stage + the S2 pre-reduction, slag removal and reducing slag making stage can be controlled to about 116 minutes, and the refining time can be controlled to about 50 minutes.
[0037] Comparative Example 1
[0038] The smelting process of this comparative example is basically as shown in the attached Figure 1 As shown, the difference from Example 1 is that there is no oxygen blowing fluxing step and reducing slag making step before the aluminum adding and steel tapping step, and the other steps are specifically as follows:
[0039] S1 Raw material melting: Load the primary material into the electric furnace before power is turned on, then turn on the power to melt, add the secondary material after 60 minutes of smelting and continue smelting, start oxygen blowing to assist melting after 90 minutes of smelting, add ferrosilicon powder into the furnace during oxygen blowing, and stop blowing oxygen after smelting for about 20 minutes.
[0040] S2 Pre-reduction, making reducing slag and tapping: After stopping oxygen blowing, add calcium carbide, carbon powder and ferrosilicon powder into the furnace to pre-reduce the slag system, and then carry out slag removal. It takes about 15 minutes from pre-reduction to the end of slag removal. After the slag removal is completed, continue to add calcium carbide, lime and other materials into the furnace to make reducing slag, and finally feed aluminum to tap steel. It takes about 43 minutes to make reducing slag and feed aluminum to tap steel.
[0041] S3 refining: After steel is tapped, the ladle is moved to the refining position for refining. During refining, lime and ferrosilicon powder are added to the refining furnace to adjust the slag system. After the slag is made, alloy is added to it according to the test results. The refining process takes about 45 minutes. Finally, the power is turned off and the refining is completed by blowing for 5 minutes. After the blowing is completed, the next step is carried out.
[0042] According to the implementation of this comparative example, the total duration of the S1 raw material melting stage + the S2 pre-reduction, slagging and reducing slag making stages is about 170 minutes, which is about 60 minutes slower than the overall process of Example 1.
[0043] Comparative Example 2
[0044] The purpose of this comparative example is to verify the effect of the feeding method on the product. The difference between this comparative example and the embodiment is that the raw material components in the primary material and the secondary material are different. Specifically: the primary material in this comparative example includes 4000kg of scrap steel, 600kg of tungsten-iron alloy, 600kg of molybdenum-iron alloy, 700kg of raw iron, 500kg of high tungsten, 3500kg of returned iron scraps and 3000kg of 6524 steel; the secondary material includes 2700kg of scrap steel, 270kg of tungsten-iron alloy, 220kg of molybdenum-iron alloy, 300kg of raw iron, 250kg of high tungsten, 1700kg of returned iron scraps and 2000kg of 6524 steel. The specific smelting steps are:
[0045] S1 Raw material melting: Load the primary material into the electric furnace before power is turned on, then turn on the power to melt, add the secondary material after 60 minutes of smelting and continue smelting, start oxygen blowing to assist melting after 90 minutes of smelting, add ferrosilicon powder into the furnace during oxygen blowing, and stop blowing oxygen after smelting for about 20 minutes.
[0046] S2 Pre-reduction, slag removal and making reducing slag: After stopping oxygen blowing, add calcium carbide, carbon powder and ferrosilicon powder into the furnace to pre-reduce the slag system, and then carry out slag removal. It takes about 15 minutes from pre-reduction to slag removal. After slag removal, continue to add calcium carbide, lime and other materials into the furnace to make reducing slag, and finally feed aluminum to tap steel. It takes about 43 minutes to make reducing slag and feed aluminum to tap steel.
[0047] S3 refining: After steel is tapped, the ladle is moved to the refining position for refining. During refining, lime and ferrosilicon powder are added to the refining furnace to adjust the slag system. After the slag is made, alloy is added to it according to the test results. The refining process takes about 45 minutes. Finally, the power is turned off and the refining is completed by blowing for 5 minutes. After the blowing is completed, the next step is carried out.
[0048] The components of the slag system are detected when oxygen blowing is stopped in S1, slag is removed in S2, and before steel is tapped in S2. The detection results are shown in Table 1 below:
[0049] Table 1: Slag composition test results
[0050]
[0051] From the above results, we can see that V 2 O 5 and Cr 2 O 3The content of V and Cr is more than 10%, indicating that there is a large amount of oxidation of V and Cr in the electric furnace smelting process. The main reason is that the 6524 steel and returned iron chips containing V and Cr are added in advance, and oxygen is blown during smelting, resulting in a large amount of oxides. When all the 6524 steel and returned iron chips are added to the secondary material, the melting time and oxygen blowing time are short after adding them, and the V in the slag system is 2 O 5 and Cr 2 O 3 The content of V and Cr is significantly reduced, which avoids the loss caused by oxidation during the oxygen blowing process, improves the recovery rate of precious metal elements, is beneficial to the control of alloy component content, and reduces production costs.
[0052] Comparative Example 3
[0053] The purpose of this comparative example is to verify the influence of aluminum addition method on the product. The difference between this comparative example and the embodiment is that aluminum wire is fed after the refining is completed, and the power is turned off and light blowing is performed for 10 minutes after the aluminum addition is completed.
[0054] The molten steel samples after the soft blowing of Example 1 and Comparative Example 3 were sampled and tested respectively. The testing method was as follows: the molten steel was extracted and processed into a metallographic sample of 110 mm × 10 mm × 10 mm, the metallographic sample was ground and polished, and the inclusions of the metallographic sample were observed and counted using an ASPEX automatic scanning electron microscope. The scanning area of each sample was about 29.6 mm 2 , automatically scans inclusions with a size of more than 1.0μm. The experimental results are shown in the attached Figure 3 and attached Figure 4 shown.
[0055] The number of inclusions detected in the steel sample of Comparative Example 3 is 43, of which the main type is alumina. The sizes of alumina inclusions are concentrated between 5μm and 10μm, and even large inclusions with a size greater than 20μm appear.
[0056] The number of inclusions detected in the steel sample of the embodiment is 25, and the main types of inclusions are aluminum oxide, magnesium aluminum oxide and calcium-containing composite inclusions. The size of aluminum oxide inclusions is mainly distributed below 4 μm, and the sizes of other inclusions are also distributed below 10 μm.
[0057] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive from any point of view. In addition, it should be understood that although this specification is described in accordance with the embodiments, it does not contain only one technical solution. This narrative of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole, and the technical solutions in the embodiments can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A high speed steel electric furnace smelting process, characterized in that: The following steps are involved: S1 Raw material melting: add primary material to the electric furnace and then turn on the power for smelting. Perform oxygen blowing to assist melting during smelting. After molten steel appears, add secondary material to the electric furnace to continue smelting and perform secondary oxygen blowing to assist melting. Add ferrosilicon powder during oxygen blowing. Adjust the power of the electric furnace and continue smelting until the secondary oxygen blowing to assist melting stops. S2 Pre-reduction, steel tapping and reducing slag making: Add reducing agent I and alloy into the furnace to pre-reduce the smelting slag system, and carry out slag removal after the pre-reduction. After the slag removal, add aluminum to tap the steel, and add reducing agent II into the ladle to make reducing slag during the tapping process; S3 refining: After slag making, the molten steel is transferred to the LF refining area for electric refining and slag-forming agent is added to adjust the refined slag system. According to the composition of the refined slag system, alloys are added to continue refining. After refining, it is gently blown and then the next process is carried out.
2. The high speed steel electric furnace smelting process according to claim 1, characterized in that: In step S1, the primary material package Including scrap steel, raw iron, high tungsten and tungsten-iron alloy, molybdenum-iron alloy; the secondary materials include returned iron filings and 6524 steel.
3. The high speed steel electric furnace smelting process according to claim 2, characterized in that: In step S1, the material is passed through After 40 to 45 minutes of electric smelting, oxygen blowing is carried out for the first time, and the time of oxygen blowing is 15 to 17 minutes. After the primary material is smelted for 60 to 65 minutes, the secondary material is added, and after the secondary material is smelted for 10 to 12 minutes, oxygen blowing is carried out for the second time, and the time of oxygen blowing is 15 to 17 minutes.
4. The high speed steel electric furnace smelting process according to claim 3, characterized in that: In step S1, the reducing agent I It comprises fluorite and calcium carbide, and the alloy comprises tungsten-iron alloy and molybdenum-iron alloy; the pre-reduction reaction time is 10 to 15 minutes.
5. A high speed steel electric furnace smelting process according to claim 1, characterized in that: In step S2, aluminum is added Add aluminum wire at a speed of 4 to 5 m / s.
6. A high speed steel electric furnace smelting process according to claim 5, characterized in that: In step S2, the reducing agent Ⅱ includes lime, calcium carbide and ferrosilicon powder, and the lime is added into the steel bag in advance.
7. A high speed steel electric furnace smelting process according to claim 1, characterized in that: The slag-forming agent in step S3 includes lime, calcium carbide and ferrosilicon powder.
8. A high speed steel electric furnace smelting process according to claim 7, characterized in that: The refined slag system in step S3 needs to meet the following indicators: basicity range 3-5; SiO2 content 10-18%; Al2O3 content 25-35%; MgO content 5-7%; (FeO+MnO) content less than 1%.
9. A high speed steel electric furnace smelting process according to claim 8, characterized in that: The alloy added in step S3 includes one or more of vanadium-iron alloy, manganese-iron alloy and chromium-containing alloy; the alloys are added in sequence at intervals of 10 minutes.