High-nitrogen steel smelting process

Through the atmospheric smelting process of electric arc furnace and LF furnace, combined with the use of multi-stage nitrogen and nitrogen alloys, the problems of high pressure and long cycle in traditional high-nitrogen steel smelting are solved, and efficient and uniform nitrogen content increase is achieved. Reduces production risks and costs and improves smelting efficiency.

CN118957398APending Publication Date: 2024-11-15WISDRI ENG & RES INC LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411067462.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The traditional high-nitrogen steel smelting process has problems such as high pressure, high risk, complex and expensive equipment and long production cycles, and the pressurized smelting method leads to uneven nitriding and long time.

Method used

The normal pressure smelting process of electric arc furnace smelting combined with LF furnace refining is adopted. The nitrogen is increased by blowing nitrogen at the bottom of the entire process. The nitrogen stirring is started in advance during the smelting of the arc furnace, and nitrogen alloy is added during the refining process to achieve multi-stage step-by-step increase. Nitrogen, shorten the nitriding period and the amount of nitride alloy used.

Benefits of technology

It has achieved high-nitrogen steel smelting with short production cycle, uniform nitriding and safe, reducing the cost and smelting risks of nitride alloys, improving production efficiency and cleanliness of the steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004981374970000031
    Figure BDA0004981374970000031
  • Figure BDA0004981374970000032
    Figure BDA0004981374970000032
  • Figure BDA0004981374970000041
    Figure BDA0004981374970000041
Patent Text Reader

Abstract

The invention discloses a high-nitrogen steel smelting process. A process route of electric arc heating (EAF), LF furnace refining (LF) and continuous casting is adopted, and the high-nitrogen steel is smelted and prepared in cooperation with a multi-stage step-by-step nitrogen increasing scheme. Initial molten steel is obtained in an electric arc furnace full-scrap-steel short-process smelting mode, a molten pool is stirred through bottom blowing nitrogen in the electric arc furnace smelting process, low-cost nitrogen is continuously introduced to replace argon in the process from tapping to refining ending, and the nitrogen plays a role in stirring the molten steel to promote inclusion floating and improving the cleanliness of the molten steel; and the retention time of nitrogen in the molten steel is prolonged, so that the nitriding reaction time is prolonged, nitriding is more uniform, and a good nitrogen increasing effect is achieved. Meanwhile, the nitriding time and the addition amount of the nitriding alloy in the refining process are saved, that is, the nitriding period is shortened, and the use cost of the nitriding alloy material is also saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to a high nitrogen steel smelting process. Background Art

[0002] In recent years, as people's research on the role of nitrogen in steel has deepened, the application value of nitrogen has also received more and more attention. The nitrogen in high-nitrogen steel has many advantages such as high strength, high toughness, high wear resistance and corrosion resistance through the comprehensive effects of solid solution strengthening, fine grain strengthening and precipitation strengthening. Its products are widely used in aviation, aerospace, medical petroleum, chemical industry, medical equipment and many other fields. In traditional metallurgical processes, high-nitrogen steel is mainly pressurized smelting, generally including hot isostatic pressing, pressurized induction, pressurized electroslag remelting and pressurized plasma melting. However, each pressurized smelting method has problems to varying degrees, such as high pressure and high risk in the production process, and the pressurized equipment is complex and expensive. At the same time, the traditional smelting method of high-nitrogen steel is relatively cumbersome, resulting in a long production cycle. Summary of the invention

[0003] The purpose of the present invention is to provide a normal pressure smelting process with short production cycle, uniform nitriding and safety.

[0004] To achieve the above object, the present invention provides a high nitrogen steel smelting process, comprising:

[0005] S1. Electric arc furnace smelting: adding scrap steel into an electric arc furnace for smelting, blowing nitrogen at the bottom for stirring during the smelting process, and obtaining a ladle;

[0006] S2. Steel tapping and ladle transfer: After steel tapping from the electric arc furnace, alloys are added to the ladle, and nitrogen is blown from the bottom throughout the process to increase the nitrogen content;

[0007] S3, refining: deoxidize the ladle in the LF furnace, add aluminum beans and nitriding alloy according to the deoxidation situation, obtain molten steel and refined slag, and continuously blow nitrogen at the bottom during the whole refining process;

[0008] S4, continuous casting: the molten steel obtained in step S3 is cast under full protection.

[0009] Furthermore, the high nitrogen steel smelting process is normal pressure smelting.

[0010] Furthermore, the amount of aluminum beans added in step S3 is 0.3-0.6 kg / t.

[0011] Furthermore, the particle size of the nitride alloy in step S3 is 4-8 mm.

[0012] Furthermore, the nitride alloy in step S3 is one or more of ferrochromium nitride, chromium nitride, ferromanganese nitride, manganese nitride, ferrovanadium nitride, vanadium nitride, ferrosilicon nitride, and silicon nitride.

[0013] Furthermore, the temperature when adding the nitriding alloy in step S3 is 1600-1630°C.

[0014] Furthermore, the refined slag obtained in step S3 has a basicity greater than 3.0 and a thickness of 50-80 mm.

[0015] The present invention adopts the process route of "electric arc heating (EAF) → LF furnace refining (LF) → continuous casting" and cooperates with a multi-stage step-by-step nitrogen increase scheme to smelt and prepare high nitrogen steel. The initial molten steel is obtained by the electric arc furnace full scrap steel short process smelting method. The electric arc furnace smelting process adopts bottom blowing nitrogen to stir the molten pool. From steel tapping to the end of refining, cheap nitrogen is continuously introduced instead of argon. Nitrogen not only stirs the molten steel to promote the floating of inclusions and improve the cleanliness of the molten steel, but also increases the residence time of nitrogen in the molten steel, thereby extending the nitriding reaction time, making the nitriding more uniform, and achieving a good nitrogen increase effect.

[0016] At the same time, compared with the prior art, the time node of nitrogen addition in the present invention is greatly advanced, and the staged nitriding solves the difficulties of high pressure, long time and uneven nitriding in the later stage. That is, nitrogen addition is started by bottom blowing nitrogen from the beginning of arc furnace smelting (C N1 ); After the steel is tapped from the electric furnace, the composition of the molten steel is adjusted by adding alloys. At this time, the molten steel already has the ability to increase nitrogen, and the time point for increasing nitrogen is greatly advanced, so that the nitrogen content in the molten steel has reached a higher level before the ladle reaches the refining position (C N2 ); in the refining process, the nitrogen content in the molten steel is finally quickly reached to the target composition requirement by adding nitriding alloy (C N3 ). Thus, the nitriding time and the amount of nitriding alloy added in the refining process can be saved, that is, while shortening the nitriding cycle, the use cost of the nitriding alloy material is also saved.

[0017] The smelting process of the high nitrogen steel is carried out under normal pressure, which can solve the high-risk problem brought about by pressurized smelting in the traditional high nitrogen steel production process. In addition, the smelting process combining nitrogen and nitrided alloys to increase nitrogen shortens the smelting cycle and improves production efficiency. DETAILED DESCRIPTION

[0018] The following detailed description of the embodiments of the present invention is intended to explain the present invention and should not be construed as limiting the present invention. In the embodiments, if specific techniques or conditions are not specified, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not specified by the manufacturer and are all conventional products that can be obtained commercially. In the following embodiments, if not clearly specified, "%" refers to weight percentage.

[0019] A high nitrogen steel smelting process

[0020] S1. Electric arc furnace smelting: adding scrap steel into an electric arc furnace for smelting, blowing nitrogen at the bottom for stirring during the smelting process, and obtaining a ladle;

[0021] Specifically, all scrap steel is melted in an electric furnace. After smelting in an electric arc furnace, the various components in the ladle are tested to determine the actual composition. Molten steel with a temperature of T1 (°C) and a weight of M0 (t) and a nitrogen content of C N1 ( The i in it is the component in the molten steel, such as carbon).

[0022] S2. Steel tapping and ladle transfer: After steel tapping from the electric arc furnace, two alloys, ferrochrome and ferromanganese, are added to the ladle, and nitrogen is blown from the bottom throughout the process to increase the nitrogen content;

[0023] Specifically, at the beginning of steel tapping in the electric arc furnace, the nitrogen flow rate at the bottom of the ladle is N1 and the nitrogen pressure is P1. When the steel tapping volume reaches 50%, according to the target composition C of the required steel grade, i , Determination of actual composition of steel ladle during steel tapping in electric arc furnace The weight of molten steel M1 (M1 is equivalent to M in formula (1)), the proportion of Cr, Mn, Mo or V in the alloy A i and yield η i Calculate and add the required alloy to the ladle. The amount of alloy added is the lower limit of the target steel grade composition, providing composition adjustment space for adding nitrogen-enhanced alloys in the refining furnace. Among them, the amount of each alloy added W i (kg) The calculation formula is:

[0024]

[0025] Among them, this formula is used to calculate the addition amount of each alloy. The recovery rate of ferromanganese, ferrochrome, ferromolybdenum and ferrovanadium is calculated at 98%, ferrosilicon is calculated at 95%, and the recovery rate of alloy carbon addition is calculated at 95% for low carbon steel and 90% for medium and high carbon steel. After all alloys are added, the weight of molten steel becomes M2.

[0026] The ladle is moved from the tapping position of the electric arc furnace to the refining position of the LF furnace. The molten steel in the ladle is blown with nitrogen from the bottom to increase the nitrogen content in the molten steel to the limit nitrogen solubility of nitrogen nitriding. At this time, the nitrogen content in the molten steel is C N2 The limiting nitrogen solubility formula for nitrogen nitriding is calculated using the following formula:

[0027]

[0028] In formula (2), is the nitrogen pressure, P is the standard atmospheric pressure, T is the tapping temperature, %N, %C, %Si, %Ni, %Mn, %Mo and %Cr are the percentages of the metal elements in the ladle. The ladle is transferred from the tapping position of the electric arc furnace to the refining position of the LF furnace, which lasts for 4-10 minutes. When it arrives at the refining position of the LF furnace, the nitrogen content of the molten steel in the ladle is C N2 .

[0029] S3, refining: deoxidize the ladle in the LF furnace, add aluminum beans and nitriding alloy according to the deoxidation situation, obtain molten steel and refined slag, and continuously blow nitrogen at the bottom during the whole refining process;

[0030] Specifically, deoxidation operation is first performed during the refining process. According to the oxygen content in the molten steel, 0.3-0.6 kg / t of aluminum beans are added during the deoxidation process to make the final oxygen content ≤ 0.0020%. During the deoxidation process, the basicity of the refined slag is ensured to be greater than 3.0 and the thickness is 50-80 mm.

[0031] After deoxidation, the required nitriding alloy is added to the furnace according to the target steel grade nitrogen content. In order to improve the nitrogen recovery rate and reduce the decomposition of the nitriding alloy, the particle size, addition time and temperature of the nitriding alloy must be strictly controlled. The nitrogen content in the nitriding alloy is B i , the nitrogen yield is ε i The nitrogen recovery rate in the nitriding alloy is calculated as ε = 80%-85%. i for:

[0032] ∑(Q i ×B i ×ε i )=(C N3 -C N2 )×M2×1000 (3).

[0033] In the above formula, C N3 is the target nitrogen content. Nitrogen is continuously blown from the bottom during the refining process. Due to the violent reaction after the addition of the nitride alloy, in order to avoid slag rolling in the molten steel, the nitrogen flow rate is set to N2 (300-600NL / min) and the pressure is set to P2 (0.8-1.0MPa) during the addition of the nitride alloy. The temperature measurement and sampling operations are completed 10-15 minutes after the addition of the nitride alloy. If the particle size of the nitride alloy is too large, the melting time will be too long, and if the particle size is too small, the nitride alloy will decompose too quickly. The particle size of chromium nitride, manganese nitride and ferrosilicon nitride should be controlled at 4-8mm to accelerate the absorption of the nitride alloy by the molten steel.

[0034] S4, continuous casting: the molten steel obtained in step S3 is cast under full protection.

[0035] Preferably, the high nitrogen steel smelting process is atmospheric pressure smelting.

[0036] Preferably, the amount of aluminum beans added in step S3 is 0.3-0.6 kg / t.

[0037] Preferably, the particle size of the nitride alloy in step S3 is 4-8 mm.

[0038] Preferably, the nitride alloy in step S3 is one or more of ferrochromium nitride, chromium nitride, ferromanganese nitride, manganese nitride, ferrovanadium nitride, vanadium nitride, ferrosilicon nitride, and silicon nitride.

[0039] Preferably, the temperature when the nitride alloy is added in step S3 is 1600-1630°C, and the temperature for adding the nitride alloy is not limited to 1600°C, 1601°C, 1602°C, 1603°C, 1604°C, 1605°C, 1606°C, 1607°C, 1608°C, 1609°C, 1610°C, 1611°C, 1612°C, 1613°C, 1614°C, 1615°C, 1616°C, 1617°C, 1618°C, 1619°C, 1620°C, 1621°C, 1622°C, 1623°C, 1624°C, 1625°C, 1626°C, 1627°C, 1628°C, 1629°C, 1630°C, etc.

[0040] Preferably, the refined slag obtained in step S3 has a basicity greater than 3.0 and a thickness of 50-80 mm.

[0041] Example 1: Smelting process of Cr17N high nitrogen steel

[0042] This implementation case is only one of the production implementation cases of high nitrogen steel and does not represent all case situations.

[0043] The high nitrogen steel smelting process in Example 1 is now used to prepare Cr17N type high nitrogen steel, and its composition is shown in Table 1. Table 1 is a target composition table of Cr17N type high nitrogen steel.

[0044] Table 1 Target composition of Cr17N type high nitrogen steel

[0045]

[0046] S1. Electric arc furnace smelting: adding scrap steel into an electric arc furnace for smelting, blowing nitrogen and stirring during the smelting process to obtain a ladle;

[0047] Specifically, all scrap steel is melted in an electric furnace with a nominal capacity of 100t. Bottom blowing nitrogen is used for stirring during the melting process, and the total bottom blowing flow rate is 90Nm 3 / h, sampling and temperature measurement before steel tapping, carbon content in molten steel Nitrogen content C N1 =0.04%, molten steel temperature T1=1620℃, molten steel weight M0=100t.

[0048] S2. Steel tapping and ladle transfer: After steel tapping from the electric arc furnace, alloys are added to the ladle, and nitrogen is blown throughout the process to increase the nitrogen content;

[0049] Specifically, when the electric furnace starts tapping steel, the nitrogen flow rate at the bottom of the ladle is N1 = 50Nm 3 / h, nitrogen pressure P1 = 1.0MPa, continuous bottom blowing nitrogen. When the steel output reaches 50%, that is, the weight of molten steel M1 = 50t, according to the target composition C of Cr17N high nitrogen steel, i , Analysis of the composition of molten steel during steelmaking in an electric arc furnace Alloy composition A i and yield η i , calculate the weight W of ferromanganese, ferrochrome and ferrosilicon to be added to the ladle by formula (1) i The amount of alloy added is the lower limit of the target composition of Cr17N high nitrogen steel, providing composition adjustment space for adding nitrogen-enhanced alloys in the refining furnace. After all alloys are added, the weight of the molten steel becomes M2.

[0050] When the ladle moves from the tapping position of the electric arc furnace to the refining position of the LF furnace, the nitrogen content in the molten steel is increased to the limit nitrogen nitriding amount by bottom blowing nitrogen. At this time, the nitrogen content in the molten steel is C N2 .

[0051] Nitrogen pressure , tapping temperature T = 1600 ° C, %N = 0.12, %C = 0.11, %Si = 0.31, %Ni = 0, %Mn = 0.4, %Mo = 0 and %Cr = 16.1. C is calculated by formula (2) N2 The ladle is transferred from the electric arc furnace to the LF furnace refining position, which lasts for 4-10 minutes. When it arrives at the LF furnace refining position, the nitrogen content of the molten steel in the ladle is C N2 =0.12%.

[0052] S3. Refining: Deoxidize the ladle in the LF furnace first, add aluminum beans and nitriding alloy according to the deoxidation situation, and obtain molten steel and refined slag. Bottom blowing of nitrogen is continued throughout the refining process.

[0053] Specifically, the temperature of the molten steel is increased to 1610-1620°C, deoxidized for 7 minutes, 30 kg of aluminum beans are added, and the basicity of the refined slag is ensured to be 3.2 and the thickness is 70 mm.

[0054] After deoxidation, according to the required nitrogen content in Cr17N high nitrogen steel, chromium nitride, manganese nitride and silicon iron nitride with a particle size of 4 mm are added into the furnace. Table 2 shows the raw material composition of the selected nitriding alloy. The addition amount Q of each nitriding alloy is calculated by formula (3): i They are (540kg chromium nitride, 50kg manganese nitride, 265kg ferrosilicon nitride):

[0055] Table 2 Nitriding alloy raw material composition (%)

[0056]

[0057] Since the reaction of nitriding alloy is violent after addition, in order to avoid slag rolling in molten steel, the nitrogen flow rate is set to N2=30Nm during the addition of nitriding alloy. 3 / h, pressure P2 = 1.0MPa. After 10-15min of adding nitriding alloy, temperature measurement and sampling are completed. After refining, the nitrogen content of molten steel is C N3 =0.165%, temperature is 1580℃.

[0058] S4, continuous casting: the molten steel obtained in step S3 is cast under full protection.

[0059] The composition and temperature of the molten steel obtained in S3 are inspected. If qualified, it is further treated with calcium, deoxidized and desulfurized according to the requirements of the steel grade, or the molten steel is directly hoisted into the continuous casting platform. In order to avoid significant fluctuations in the nitrogen content in the molten steel, the continuous casting process adopts full-process protective pouring to ensure the stability of the chemical composition of the finished steel grade, including the nitrogen content.

[0060] After pouring, the composition of the ingot was tested, and the obtained composition is shown in Table 3. All the components of the ingot meet the target composition range requirements.

[0061] Table 3 Composition of ingot steel grades

[0062]

[0063] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.

Claims

1. A high nitrogen steel smelting process, characterized in that: include: S1. Electric arc furnace smelting: adding scrap steel into an electric arc furnace for smelting, blowing nitrogen at the bottom for stirring during the smelting process, and obtaining a ladle; S2. Steel tapping and ladle transfer: After steel tapping from the electric arc furnace, alloys are added to the ladle, and nitrogen is blown from the bottom throughout the process to increase the nitrogen content; S3, refining: deoxidize the ladle in the LF furnace, add aluminum beans and nitriding alloy according to the deoxidation situation, obtain molten steel and refined slag, and continuously blow nitrogen at the bottom during the whole refining process; S4, continuous casting: the molten steel obtained in step S3 is cast under full protection.

2. The high nitrogen steel smelting process according to claim 1, characterized in that: The high nitrogen steel smelting process is normal pressure smelting.

3. The high nitrogen steel smelting process according to claim 1, characterized in that: The amount of aluminum beans added in step S3 is 0.3-0.6 kg / t.

4. The high nitrogen steel smelting process according to claim 1, characterized in that: The particle size of the nitrided alloy in step S3 is 4-8 mm.

5. The high nitrogen steel smelting process according to claim 1, characterized in that: The nitride alloy in step S3 is one or more of ferrochromium nitride, chromium nitride, ferromanganese nitride, manganese nitride, ferrovanadium nitride, vanadium nitride, ferrosilicon nitride, and silicon nitride.

6. The high nitrogen steel smelting process according to claim 1, characterized in that: The temperature when adding the nitriding alloy in step S3 is 1600-1630°C.

7. The high nitrogen steel smelting process according to claim 1, characterized in that: The refined slag obtained in step S3 has a basicity greater than 3.0 and a thickness of 50-80 mm.