Reagent MP136 for extracting molybdenum from copper smoke dust leachate as well as preparation method and application of reagent MP136

By extracting the molybdenum reagent MP136 from copper smoke leaching liquid prepared by sodium cellulose, glycerol and EDC, and oscillation extraction with sulfonated kerosene, the problem of low molybdenum recovery in the molybdenum method is solved, and high-efficiency molybdenum separation is achieved and treatment is reduced. Cost and reduce resource waste and environmental pollution.

CN118957259APending Publication Date: 2024-11-15KUNMING METALLURGY INST
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411084657.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The recovery rate of molybdenum in the molybdate process is concentrated between 70 and 90%, which fails to achieve efficient recycling of molybdenum, and has high processing costs and complex processes, which poses the risk of resource waste and environmental pollution.

Method used

The molybdenum reagent MP136 was extracted from copper smoke leaching liquid prepared by sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carboyldiimide (EDC), and was formed by pressurized reaction in highly acidic wastewater. Anionic composite extractant, combined with sulfonated kerosene, is used for oscillation extraction, to achieve efficient separation of molybdenum.

Benefits of technology

The extraction rate of molybdenum in highly acidic wastewater reaches 85-95%, reducing treatment costs, simplifying the process flow, improving the recycling efficiency of molybdenum, and reducing resource waste and environmental pollution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a reagent MP136 for extracting molybdenum from copper smoke dust leachate as well as a preparation method and application of the reagent MP136. The reagent MP136 for extracting the molybdenum from the copper smoke dust leachate is prepared by taking sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) as raw materials. The preparation method comprises the step of carrying out pressurized reaction on the sodium cellulose, the glycerol and the 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) according to a formula ratio in an oxygen atmosphere.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy and chemical industry, and specifically relates to a copper fume leaching solution to extract molybdenum reagent MP136 and a preparation method and application thereof. Background Art

[0002] Molybdenum is found in small quantities on Earth, accounting for only 0.1% of the mass of the earth's crust, and is a rare precious metal. At the same time, molybdenum is a non-renewable resource and also a strategic resource. Due to its small expansion coefficient, high electrical conductivity, and good thermal conductivity, it is widely used in the steel industry, non-ferrous metals, chemical industry and other fields, and has become an irreplaceable strategic material in the national economy. my country has an advantage in molybdenum resources, and its molybdenum ore reserves rank second in the world. However, with the continuous expansion and development of the application of molybdenum resources in high-tech and other fields, the demand for molybdenum and its metal products has also increased year by year. Therefore, molybdenum production companies are very optimistic about the recovery rate of molybdenum, thereby demonstrating the strength of the company and creating greater benefits.

[0003] With the increase in demand for molybdenum, the molybdenum acid extraction process has developed rapidly, and its separation and purification methods include precipitation, ion exchange, extraction, activated carbon adsorption, etc. The separated molybdenum-containing solution is subjected to the traditional acid precipitation process and concentrated crystallization process to obtain the molybdenum product. The acidic wastewater after the precipitate is separated by the two precipitation processes contains a large amount of molybdenum metal and heavy metal impurities such as Cu and Pb. During the circulation of wastewater, precipitates will block the pipeline and cause equipment corrosion. If not treated, it will not only cause environmental pollution, but also cause serious waste of resources. Therefore, the treatment of acidic wastewater in molybdenum hydrometallurgy and the recovery of molybdenum have certain economic benefits and significant social benefits.

[0004] Common molybdenum recovery technologies for ammonium molybdate production wastewater abroad include activated carbon adsorption, extraction, ion exchange and inorganic salt processes. A foreign ammonium molybdate production company added (NH4)2S to the acidic wastewater of ammonium molybdate and stirred it at about 70℃ for 30 minutes, and MoS2 was precipitated, with a molybdenum recovery rate of more than 90%. Kazuo Ise and others from the Japan Pollution Resources Research Institute studied the use of pH 1.46 in a 2g / L molybdenum solution and activated carbon adsorption at 25℃, and the molybdenum residual rate was 30%.

[0005] Domestic research institutes such as Guilin use alkali to adjust the acidic waste liquid to precipitate Cu and Zn ions. These precipitates absorb and wrap MoO4 2- The formation of co-precipitation makes molybdenum sink into the slag, and 95% of molybdenum can be recovered. Tang Lixia et al. used a nanofiltration membrane system to treat the acidic wastewater from ammonium molybdate production, and the retention rate of molybdenum reached more than 80-95%. Liu Minjie et al. dynamically treated the acidic wastewater through DK resin and HA resin, and 86-92% of molybdenum and 98% of copper were recovered. However, these methods have high processing costs and complex processes, and the recovery rate of molybdenum is concentrated between 70% and 90%, and efficient recycling of molybdenum is not achieved.

[0006] Therefore, it is very necessary to develop a molybdenum extraction reagent and a recovery method that can solve the above-mentioned technical problems. Summary of the invention

[0007] The first purpose of the present invention is to provide a copper fume leaching solution for extracting molybdenum reagent MP136; the second purpose is to provide a preparation method of the copper fume leaching solution for extracting molybdenum reagent MP136; the third purpose is to provide an application of the copper fume leaching solution for extracting molybdenum reagent MP136.

[0008] The first object of the present invention is achieved in that the copper dust leachate molybdenum extraction reagent MP136 is prepared using sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) as raw materials.

[0009] The second object of the present invention is achieved by subjecting sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a prescribed ratio to a pressure reaction under an oxygen atmosphere to prepare the product.

[0010] The specific operation is as follows: sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) are pressurized and reacted for 1-4 hours at an oxygen pressure of 1.2-1.5 kPa and a temperature of 150-200°C, and then filtered and separated to obtain a composite extractant MP136 for extracting molybdenum; wherein the molar ratio of sodium cellulose, glycerol and EDC is 1:2-50:1-15. The extractant has stable extraction performance for molybdenum under high acid and high temperature conditions.

[0011] The third object of the present invention is achieved by using the copper fume leaching solution to extract molybdenum reagent MP136 in a process for recovering molybdenum from highly acidic wastewater.

[0012] The technical principle of extracting molybdenum reagent MP136 from copper fume leaching solution of the present invention is: under the dispersing effect of sodium cellulose, -OH in glycerol combines with propyl in 1-ethyl-(3-dimethylaminopropyl)carbodiimide to form anionic valence bonds, i.e. MP136 anionic composite extractant, and Mo ions in the solution combine with anions of MP136 to form molybdenum-amino chelates, thereby achieving separation of molybdenum from copper, zinc, arsenic and antimony in the solution. DETAILED DESCRIPTION

[0013] The present invention is further described below in conjunction with the embodiments, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.

[0014] The copper dust leaching solution molybdenum extraction reagent MP136 of the present invention is prepared by using sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) as raw materials.

[0015] The molar ratio of sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) is 1:(2-50):(1-15).

[0016] The preparation method of the copper fume leaching solution for extracting molybdenum reagent MP136 is prepared by subjecting sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a prescribed ratio to a pressure reaction under an oxygen atmosphere.

[0017] The oxygen pressure of the pressurized reaction is 1.2~1.5KPa.

[0018] The temperature of the pressurized reaction is 150-200°C.

[0019] The time of the pressurized reaction is 1 to 4 hours.

[0020] The application of the copper dust leaching solution to extract the molybdenum reagent MP136 described in the present invention is the application of the copper dust leaching solution to extract the molybdenum reagent MP136 in the process of recovering molybdenum in highly acidic wastewater.

[0021] The application of the copper dust leaching solution molybdenum extraction reagent MP136 in the process of recovering molybdenum from highly acidic wastewater is to add sulfonated kerosene to the copper dust leaching solution molybdenum extraction reagent MP136, mix them evenly, and then oscillate and extract the molybdenum-containing dust leaching solution.

[0022] The volume ratio of the copper fume leaching solution to extract molybdenum reagent MP136 and sulfonated kerosene is (15-40): (60-85).

[0023] The molybdenum content in the copper fume leaching solution is 1-20 g / L.

[0024] The oscillation frequency is 150-200 r / min, and the oscillation time is 10-30 min.

[0025] The present invention is further described below with specific implementation cases: Example 1 Cellulose sodium, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a molar ratio of 1:25:8 were pressurized and reacted at an oxygen pressure of 1.2-1.5 KPa and a temperature of 180-200°C for 1 hour, and the copper fume leaching solution molybdenum extraction reagent MP136 was prepared by filtration and separation.

[0026] Example 2 Sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a molar ratio of 1:2:1 were pressurized and reacted for 4 hours at an oxygen pressure of 1.2-1.5 KPa and a temperature of 150-180°C. The copper fume leaching solution molybdenum extraction reagent MP136 was prepared by filtration and separation.

[0027] Example 3 Sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a molar ratio of 1:50:15 were pressurized and reacted at an oxygen pressure of 1.2-1.5 KPa and a temperature of 160-180°C for 3 hours, and the copper fume leaching solution molybdenum extraction reagent MP136 was prepared by suction filtration and separation.

[0028] Example 4 Sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a molar ratio of 1:10:10 were pressurized and reacted for 2 hours at an oxygen pressure of 1.2-1.5 KPa and a temperature of 170-190°C. The copper fume leaching solution molybdenum extraction reagent MP136 was prepared by suction filtration and separation.

[0029] Example 5 Cellulose sodium, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a molar ratio of 1:35:7 were pressurized and reacted at an oxygen pressure of 1.2-1.5 KPa and a temperature of 170-180°C for 2.5 hours, and the copper fume leaching solution molybdenum extraction reagent MP136 was prepared by filtration and separation.

[0030] Example 6 The copper fume leaching solution prepared in Example 1 was used to extract the molybdenum reagent for testing, as follows: Correctly measure 15~40% volume fraction of copper smoke leaching solution to extract molybdenum reagent MP136 + 60~85% sulfonated kerosene, mix them evenly, and extract the molybdenum-containing smoke leaching solution containing Mo 1-20g / L. The ratio O / A is 1:1-4, the oscillation frequency is 150-200r / min, and the oscillation is performed at room temperature for 10-30min. After the reaction stops, the organic phase and the aqueous phase are separated, and the molybdenum extraction rate reaches 85-95%.

[0031] Example 7 The copper fume leaching solution prepared in Example 2, Example 3, Example 4, and Example 5 were respectively used to extract the molybdenum reagent MP136, and the method was the same as that in Example 6. The results all showed that the copper fume leaching solution extracted molybdenum reagent MP136 of the present invention had an extraction rate of 85-95% for molybdenum.

Claims

1. A copper dust leaching solution for extracting molybdenum reagent MP136, characterized in that: The copper dust leaching solution molybdenum extraction reagent MP136 is prepared using sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) as raw materials.

2. The copper fume leaching solution extraction molybdenum reagent MP136 according to claim 1, characterized in that: The molar ratio of sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) is 1:(2-50):(1-15).

3. A method for preparing the molybdenum reagent MP136 extracted from copper fume leaching solution according to 1 or 2, characterized in that: The invention is prepared by subjecting sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) with a certain formula to a pressure reaction under an oxygen atmosphere.

4. The preparation method according to claim 3, characterized in that: The oxygen pressure of the pressurized reaction is 1.2~1.5KPa.

5. The preparation method according to claim 3, characterized in that: The temperature of the pressurized reaction is 150-200°C.

6. The preparation method according to claim 3, characterized in that: The time of the pressurized reaction is 1 to 4 hours.

7. An application of the copper fume leaching solution according to claim 1 or 2 to extract molybdenum reagent MP136, characterized in that: The copper fume leaching solution is used to extract the molybdenum reagent MP136 in the process of recovering molybdenum from highly acidic wastewater.

8. The use according to claim 7, characterized in that: The application of the copper dust leaching solution molybdenum extraction reagent MP136 in the process of recovering molybdenum from highly acidic wastewater is to add sulfonated kerosene to the copper dust leaching solution molybdenum extraction reagent MP136, mix them evenly, and then oscillate and extract the molybdenum-containing dust leaching solution.

9. The use according to claim 8, characterized in that: The volume ratio of the copper fume leaching solution to extract molybdenum reagent MP136 and sulfonated kerosene is (15-40): (60-85).

10. The use according to claim 8, characterized in that: The oscillation frequency is 150-200 r / min, and the oscillation time is 10-30 min.

Citation Information

Cited By

  • Preparation method of molybdenum extraction agent for copper smelting tailing leachate