Method for extracting lithium from waste electrolyte and recycling lithium
By grafting crown ethers onto adsorption resins and optimizing the component ratio, combined with the specific pore structure of the crown ethers and the resin matrix, the problems of insufficient selectivity and capacity of adsorbents in existing lithium-ion battery recycling have been solved, achieving efficient recovery of high-purity lithium and simplifying the process.
Patent Information
- Application Number
- CN202411450322.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-17
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-10-17
AI Technical Summary
In existing lithium-ion battery recycling technologies, the selectivity, adsorption capacity, and mass transfer rate of adsorbents are low, making it difficult to achieve efficient recovery of high-purity lithium. Furthermore, existing processes are complex and difficult to industrialize.
Adsorption resin grafted with crown ethers was used as a specific lithium adsorbent. By optimizing the component ratio and grafting method during the preparation process, and combining the specific pore structure of the crown ether and the resin matrix, the adsorption selectivity and capacity of lithium ions were improved, and high-purity lithium was obtained through subsequent processing.
It achieves the recovery of high-purity lithium with a high recovery rate, simplifies the process flow, adapts to environmental changes, and improves the stability and adsorption capacity of the adsorbent.
Smart Images

Figure CN118957276A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion battery recycling, and specifically relates to a method for extracting lithium from waste electrolyte and recycling it. Background Art
[0002] The rapid development of new energy technologies is leading the transformation of the global energy structure. As a key technology, lithium-ion batteries have been successfully commercialized and widely used in many fields. Especially in new energy fields such as electric vehicles and energy storage systems, lithium-ion batteries have become an indispensable energy storage solution due to their advantages such as high energy density, long cycle life and fast charging capability. However, with the continuous expansion of lithium-ion battery installed capacity, the amount of waste lithium-ion batteries is also increasing year by year, bringing new environmental challenges.
[0003] If waste lithium-ion batteries are not properly handled after being discarded, the heavy metals such as lithium, cobalt, nickel, etc., as well as solvents and other organic auxiliary materials contained in them may cause serious pollution to the soil, water sources and other environments. At the same time, the recycling and reuse of waste lithium-ion batteries has important economic and environmental value. Since the metal resources contained in these batteries have limited reserves in nature and are expensive in the market, recycling these metals can not only reduce the demand for mining new mineral resources and reduce mining costs, but also reduce damage to the environment. In addition, secondary pollution control and material recycling during the recycling process are also important components for achieving sustainable development and a circular economy.
[0004] The recycling and treatment technologies for waste lithium-ion batteries mainly include three methods: physical separation, biochemical treatment, and chemical treatment. Physical separation includes flotation and grinding. Biochemical treatment uses microorganisms to decompose and metabolize battery materials and selectively leach specific elements, but it is still very immature and has no practical application. Chemical treatment is currently a widely used recycling and treatment method, and there are many related studies. It is mainly divided into three categories: pyrometallurgical process, hydrometallurgical process and electrode regeneration.
[0005] At present, the main methods for lithium-ion battery recovery and extraction include precipitation, membrane separation, adsorption, etc. During precipitation, other metal ions are often co-precipitated, which increases the difficulty of separation and the cost. The membrane separation method also faces the problems of membrane pollution and long separation time. The adsorption method has the advantages of lower cost, less environmental pollution, high extraction rate and easy continuous operation, but the selectivity, adsorption capacity and mass transfer rate of common adsorbents still need to be further improved. Therefore, according to Li + The structural characteristics of Li + Based on the interaction with adsorbent adsorption sites, new adsorbents are studied and used to obtain high-purity Li + Extremely important.
[0006] Crown ethers containing 12-14 ring members are good Li + Selective ligands. Currently, related studies have selected 12-14-membered crown ethers as Li + Selective ligands, using high internal phase surfaces to copolymerize or surface modify Li + Fixation of ligands, such as Chinese patent document CN110227424A discloses a preparation method and application of a covalently modified high-density crown ether functionalized porous adsorbent; the steps are: first prepare a porous polymer PVBC and a porous polymer with surface branched poly(glycidyl methacrylate), recorded as PVBC-g-PGMA; mix PVBC-g-PGMA and DMF, and add 2AB12C4 after PVBC-g-PGMA is dispersed in DMF; after a water bath reaction, the obtained product is washed with DMF, ethanol, and double distilled water in turn, and after vacuum drying, an aminoethylbenzo-12-crown-4 modified porous adsorbent is obtained; the porous adsorbent prepared by the invention effectively improves the adsorption capacity and mass transfer efficiency, solves the problems of low density of action sites and deep embedding of action sites of existing lithium extraction adsorbents, and provides a new idea for the development of efficient lithium extraction adsorbents.
[0007] However, although these materials have good Li + However, on the one hand, its process is relatively complicated and difficult to apply industrially; on the other hand, its adsorption selectivity and adsorption capacity for lithium ions still need to be further improved. Summary of the invention
[0008] In order to solve the problems existing in the background technology, the present invention provides a method for extracting and recycling lithium from waste electrolytes. The present invention adopts an adsorption resin grafted with crown ether as a specific lithium adsorbent, which can obtain a higher lithium element recovery rate and purity, and the lithium element can be recycled through subsequent process processing.
[0009] An object of the present invention is to provide a method for extracting lithium from waste electrolyte, which specifically comprises the following steps: S1: discharging and disassembling the lithium battery to obtain positive electrode waste; adding sodium hydroxide to soak, the liquid-solid ratio of sodium hydroxide to positive electrode waste is 3-10:1, and filtering to obtain positive electrode powder; S2: The positive electrode powder is leached with sulfuric acid with a concentration of 0.3-0.5 mol / L and 30% hydrogen peroxide, and the leaching solution and leaching residue are obtained after filtering; Preferably, in order to help improve the recovery rate and purity of lithium ions, the present invention further includes the step of adjusting the pH value of the system to 8.5 after the acid leaching process, and filtering after precipitation, the purpose of which is to remove impurity ions and increase the lithium content of the leachate.
[0010] S3: passing the leaching solution through a resin column using an adsorption resin grafted with crown ether as an adsorption medium at a flow rate of 2 BV / h, detecting the lithium content in the effluent, and stopping eluting when the lithium content in the effluent is greater than 0.1 ug / L; At this point, the resin column is in an adsorption saturation state.
[0011] The adsorption resin grafted with crown ether is prepared by the following method: The resin precursor is prepared by conventional suspension polymerization with glycidyl methacrylate (GMA), triallyl isocyanurate (TAIC), azobisisobutyronitrile and n-heptane as oil phase, water and polyvinyl alcohol as aqueous phase, and the mass ratio of aqueous phase to oil phase is 3:1; the resin precursor is added to a mixed solution of 2-hydroxymethyl-12-crown-4 and sodium hydride, refluxed under nitrogen atmosphere, and dried to obtain a crown-etherified adsorption resin; the crown-etherified adsorption resin is subjected to epoxy ring opening with ethylenediamine, filtered, washed, and dried to obtain the adsorption resin grafted with the crown ether; S4: Desorbing the resin with dilute hydrochloric acid to obtain a lithium-containing solution.
[0012] Furthermore, in step S1, the liquid-to-solid ratio of sodium hydroxide to the cathode waste is 10:1.
[0013] Furthermore, the specific conditions of step S2 are: adding the positive electrode powder obtained in step S1 to a dilute sulfuric acid solution with a concentration of 0.3-0.5 mol / L at a liquid-to-solid ratio of 20 mL-30 mL: 1 g to extract lithium, wherein 1 mL of 30% hydrogen peroxide is added to the dilute sulfuric acid solution; leaching at 55-65° C. for 120-200 min, adjusting the pH value of the system to 8.5, filtering, and obtaining a leachate and a leach residue.
[0014] Furthermore, in step S3, the rotation speed of the suspension polymerization is 260 r / min, the mass ratio of GMA to TAIC in the oil phase is 5:1, and the mass ratio of n-heptane to GMA is 1:3.
[0015] Furthermore, in step S3, the heating rate of the suspension polymerization is to stir until the particle size is uniform, then heat to 85° C. at a rate of 2° C. / min, and keep warm for 4 hours.
[0016] Further, the crown etherified adsorption resin described in step S3 is prepared by the following method: 2-Hydroxymethyl-12-crown-4 and sodium hydride were mixed in a molar ratio of 1:1 to obtain a mixed solution, which was stirred at 55°C for 6 hours under a nitrogen atmosphere. The resin precursor was added to the mixed solution, and the mass ratio of the resin precursor to 2-hydroxymethyl-12-crown-4 was 6:1. The mixture was refluxed for 70 hours under nitrogen protection, filtered, washed, and dried to obtain a crown-etherified adsorption resin.
[0017] Furthermore, the specific process conditions for the epoxy ring opening using ethylenediamine in step S3 are: Take the crown etherified adsorption resin, soak it in DMF, fully swell for 24 hours, add ethylenediamine in a mass ratio of 1:5 of crown etherified resin: ethylenediamine, and react at 70° C. for 5 hours. After the reaction is completed, cool, filter, wash, and dry to obtain the adsorption resin grafted with crown ether.
[0018] Furthermore, the specific process of step S4 is: after disassembling the resin column after adsorption in step S3, immersing it in 1 mol / L dilute hydrochloric acid, the liquid-solid ratio of resin to dilute hydrochloric acid is 1:36-40, and shaking and stirring at 25° C. for 4-6 hours to obtain a lithium-containing solution.
[0019] Another object of the present invention is to provide a method for recycling lithium after extracting it from waste electrolyte, characterized in that battery-grade lithium carbonate can be obtained by adding sodium carbonate to a lithium-containing solution.
[0020] It should be noted that it is well known in the art that it is difficult to form lithium carbonate products under acidic conditions. In the process of preparing lithium carbonate, the present invention needs to add an alkali agent commonly used in the art to adjust the pH of the system to between 7 and 11, and then add carbonate to carry out the preparation process of lithium carbonate. Its role has two aspects. One is that it can neutralize excess acid in the lithium-containing solution. The other is that it is more conducive to the formation of lithium carbonate under alkaline conditions, thereby improving the final purity of the lithium carbonate product. The alkali agent described in the present invention can be an alkali agent commonly used in the art, such as sodium hydroxide.
[0021] The present invention has the following beneficial effects: 1. The present invention relies on Li + In view of the structural differences between the adsorption capacity and adsorption selectivity of lithium, glycidyl methacrylate is used as a monomer, triallyl isocyanurate is used as a polymerization cross-linking agent, and n-heptane is used as a porogen. By adopting an optimized component ratio, a precursor resin with a suitable pore size distribution can be obtained. The rich pore structure in the precursor resin can help improve the adsorption capacity and adsorption selectivity of lithium to a certain extent during the elution process.
[0022] 2. The present invention grafts 2-hydroxymethyl-12-crown-4 onto the precursor resin, so that the crown ether group is retained in the resin precursor. The crown ether has an electron-rich cavity, and its cavity size is similar to that of Li + The diameters are relatively close, and they can form very stable complexes with lithium ions. They have high resistance to ion interference and have specific selective adsorption for lithium ions. In addition, the synthesis conditions of the present invention are more stable and can adapt to environmental changes. The surface contains more groups and has a relatively high adsorption capacity.
[0023] 3. After 2-hydroxymethyl-12-crown-4 is grafted onto the precursor resin, the epoxy groups wrapped in the resin matrix are fully exposed through sufficient swelling, and then ethylenediamine is used as a functionalizing agent to open the epoxy ring, so that a certain number of amino groups can be introduced into the resin matrix. The hydrogen ions generated when the crown ether groups on the resin matrix specifically adsorb lithium can be combined with the amino groups in the resin matrix, thereby further improving the resin's adsorption capacity for lithium ions; that is, the present invention further improves the resin's adsorption capacity and adsorption selectivity for lithium ions by utilizing the coordination among the crown ether, the amino group and the specific pore structure in the resin matrix, and is applied to the recovery of lithium elements from lithium-ion battery positive electrode materials, thereby obtaining high-purity lithium with a high lithium recovery rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a SEM spectrum of the adsorption resin grafted with crown ether prepared in the present invention; Figure 2 This is the pore size distribution diagram of the adsorption resin grafted with crown ether prepared in the present invention. DETAILED DESCRIPTION
[0025] The present invention is described in detail below in conjunction with specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments. Based on the given embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application. It should be noted that the adsorption resin grafted with crown ether described in the following Examples 1-3 is prepared in the following manner: Add 1000g of water phase (including 10g of 5% polyvinyl alcohol and the rest of deionized water) into a three-necked flask, stir evenly, heat to 40°C, add oil phase at a mass ratio of 3:1 between water phase and oil phase (the polymerized monomer GMA:TAIC in the oil phase is 5:1, the initiator is azobisisobutyronitrile, the porogen is n-heptane, and the mass ratio of n-heptane to GMA is 1:3), stir at a speed of 260 rpm, and after the particle size is uniform, heat to 85°C at a rate of 2°C / min, keep warm for 4h, filter, extract with petroleum ether as solvent for 12h, remove the solvent, and dry to obtain a resin precursor.
[0026] 2-Hydroxymethyl-12-crown-4 and sodium hydride were mixed in a molar ratio of 1:1, stirred at 55°C for 6 hours, and the stirring was carried out under a nitrogen atmosphere. The resin precursor was added to the above solution, and the mass ratio of the resin precursor to 2-hydroxymethyl-12-crown-4 was 6:1. The mixture was refluxed for 70 hours under nitrogen protection, filtered, washed, and dried to obtain a crown-etherified adsorption resin.
[0027] Take the crown etherified adsorption resin, soak it in DMF, fully swell for 24 hours, add ethylenediamine at a mass ratio of 1:5 and react at 70° C. for 5 hours. After the reaction is completed, cool, filter, wash, and dry to obtain the adsorption resin grafted with the crown ether.
[0028] The morphology of the prepared adsorption resin grafted with crown ether was characterized by scanning electron microscopy. Figure 1 shown.
[0029] The specific surface area and pore analysis were determined by low temperature (77K) nitrogen adsorption and desorption method. The sample was pretreated with high-purity nitrogen before the measurement, and the treatment condition was 120ºC purge for 13h. The BELSORP-mini II adsorption instrument measured the adsorption and degassing isotherms of nitrogen at 77K, and automatically calculated the average pore size of the resin to be 6.9nm and the specific surface area to be 1025m 2 / g.
[0030] The present invention measures the content of amino groups in the resin by hydrochloric acid titration. After detection, the content of amino groups in the adsorption resin grafted with crown ethers is 1.6 mmol / g.
[0031] The content of crown ether in the resin was measured by gas chromatography-mass spectrometry (GC-MS). The results showed that the content of crown ether in the adsorption resin grafted with crown ether was 3.1 mmol / g.
[0032] The lithium-ion battery is mainly composed of a negative electrode sheet, a separator, and a positive electrode sheet, wherein the positive electrode sheet uses aluminum foil as a current collector and is coated with positive electrode materials (active material + conductive agent + binder PVDF) on both sides. It should be noted that the Li content of the waste lithium-ion battery positive electrode material used in the following embodiments is 7.4%, the Ni content is 20.1%, the Co content is 19.8%, and the Mn content is 21.3%.
[0033] Example 1 S1: Discharge and disassemble the lithium battery to obtain positive electrode waste; add sodium hydroxide to soak, and the liquid-solid ratio of sodium hydroxide to positive electrode waste is 3:1, and then filter to obtain positive electrode powder.
[0034] S2: The positive electrode powder obtained in step S1 is added to a 0.3 mol / L dilute sulfuric acid solution at a liquid-to-solid ratio of 20 mL: 1 g to extract lithium, and 1 mL of 30% hydrogen peroxide is added to the dilute sulfuric acid solution; leaching is performed at 60° C. for 180 min, the pH value of the system is adjusted to 8.5, and then filtered to obtain a leachate and a leach residue.
[0035] S3: The leachate is passed through an adsorption column using an adsorption resin grafted with crown ether as an adsorption medium at a flow rate of 2BV / h, and the lithium content in the effluent is detected. When the lithium content in the effluent is greater than 0.1ug / L, elution is stopped. At this time, the resin is in an adsorption saturation state.
[0036] S4: disassemble the resin column after adsorption saturation in step S3, soak it in 1 mol / L dilute hydrochloric acid, the solid-liquid ratio of the resin to the dilute hydrochloric acid is 1:36, and shake and stir at 25° C. for 4 hours to obtain a lithium-containing solution.
[0037] Example 2 S1: Discharge and disassemble the lithium battery to obtain positive electrode waste; add sodium hydroxide for soaking, and obtain positive electrode powder after filtration with a liquid-solid ratio of sodium hydroxide to positive electrode waste of 5:1.
[0038] S2: The positive electrode powder obtained in step S1 is added to a 0.5 mol / L dilute sulfuric acid solution at a liquid-to-solid ratio of 25 mL: 1 g to extract lithium, and 1 mL of 30% hydrogen peroxide is added to the dilute sulfuric acid solution; leaching is performed at 55° C. for 200 min, the pH value of the system is adjusted to 8.5, and then filtered to obtain a leachate and a leach residue.
[0039] S3: The leachate is passed through an adsorption column using an adsorption resin grafted with crown ether as an adsorption medium at a flow rate of 2BV / h, and the lithium content in the effluent is detected. When the lithium content in the effluent is greater than 0.1ug / L, elution is stopped. At this time, the resin is in an adsorption saturation state.
[0040] S4: disassemble the resin column after adsorption saturation in step S3, soak it in 1 mol / L dilute hydrochloric acid, the solid-liquid ratio of the resin to the dilute hydrochloric acid is 1:40, and shake and stir at 25° C. for 5 hours to obtain a lithium-containing solution.
[0041] Example 3 S1: Discharge and disassemble the lithium battery to obtain positive electrode waste; add sodium hydroxide for soaking, and obtain positive electrode powder after filtration with a liquid-solid ratio of sodium hydroxide to positive electrode waste of 10:1.
[0042] S2: The positive electrode powder obtained in step S1 is added to a 0.3 mol / L dilute sulfuric acid solution at a liquid-to-solid ratio of 30 mL: 1 g to extract lithium, and 1 mL of 30% hydrogen peroxide is added to the dilute sulfuric acid solution; leaching is performed at 65° C. for 120 min, the pH value of the system is adjusted to 8.5, and then filtered to obtain a leachate and a leach residue.
[0043] S3: The leachate is passed through an adsorption column using an adsorption resin grafted with crown ether as an adsorption medium at a flow rate of 2BV / h, and the lithium content in the effluent is detected. When the lithium content in the effluent is greater than 0.1ug / L, elution is stopped. At this time, the resin is in an adsorption saturation state.
[0044] S4: After the resin column is saturated with adsorption in step S3, it is disassembled and immersed in 1 mol / L dilute hydrochloric acid, with a solid-liquid ratio of the resin to the dilute hydrochloric acid of 1:40, and the mixture is shaken and stirred at 25° C. for 6 h to obtain a lithium-containing solution.
[0045] Comparative Example 1 The adsorption resin grafted with crown ether described in this comparative example was prepared by the following method: Add 1000g of water phase (including 10g of 5% polyvinyl alcohol and the rest of deionized water) into a three-necked flask, stir evenly, heat to 40°C, add oil phase at a mass ratio of 3:1 between water phase and oil phase (the polymerized monomer GMA:TAIC in the oil phase is 5:1, the initiator is azobisisobutyronitrile, the porogen is n-heptane, and the mass ratio of n-heptane to the polymerized monomer is 1:3), stir at a speed of 260 rpm, heat to 85°C at a rate of 2°C / min, keep warm for 4h, filter, remove the solvent by Soxhlet extraction with petroleum ether as solvent, and dry to obtain a resin precursor.
[0046] 2-Hydroxymethyl-12-crown-4 and sodium hydride were mixed in a molar ratio of 1:1, stirred at 55°C for 6 hours, and the stirring was carried out under a nitrogen atmosphere. The resin precursor was added to the above solution, and the mass ratio of the resin precursor to 2-hydroxymethyl-12-crown-4 was 6:1. The mixture was refluxed for 70 hours under nitrogen protection, filtered, washed, and dried to obtain a crown-etherified adsorption resin.
[0047] The specific process conditions for recovering lithium element in this comparative example are as follows: S1: discharging and disassembling the lithium battery to obtain positive electrode waste; adding sodium hydroxide to soak, and filtering to obtain positive electrode powder after the liquid-solid ratio of sodium hydroxide to positive electrode waste is 5:1; S2: The positive electrode powder obtained in step S1 is added to a 0.5 mol / L dilute sulfuric acid solution at a liquid-to-solid ratio of 25 mL: 1 g to extract lithium, and 1 mL of 30% hydrogen peroxide is added to the dilute sulfuric acid solution; leaching is performed at 55° C. for 200 min, the pH value of the system is adjusted to 8.5, and then filtered to obtain a leachate and a leach residue.
[0048] S3: The leachate is passed through an adsorption column using crown etherified adsorption resin as the adsorption medium at a flow rate of 2BV / h, and the lithium content in the effluent is detected. When the lithium content in the effluent is greater than 0.1ug / L, elution is stopped. At this time, the resin is in an adsorption saturation state.
[0049] S4: After the resin column is saturated with adsorption in step S3, it is disassembled and immersed in 1 mol / L dilute hydrochloric acid, with the solid-liquid ratio of the resin to the dilute hydrochloric acid being 1:40, and the mixture is shaken and stirred at 25° C. for 5 h to obtain a lithium-containing solution.
[0050] The lithium content and recovery rate related indicators before and after treatment with the adsorption resin grafted with crown ether in the embodiments and comparative examples are shown in the following table: Examples and Comparative Examples Example 1 Example 2 Example 3 Comparative Example 1 Lithium content in leachate (%) 38.3 36.9 38.6 36.9 Lithium content of analytical solution (%) 95.3 96.8 96.7 87.6 Lithium recovery rate (%) 95.6 98.7 97.3 88.9 By comparing the data of the embodiments and the comparative examples, it can be seen that in embodiments 1-3, after 2-hydroxymethyl-12-crown-4 is grafted on the precursor resin, the epoxy groups wrapped in the resin matrix are fully exposed through sufficient swelling, and then the epoxy is ring-opened with ethylenediamine as a functionalizing agent, and a certain number of amino groups can be introduced into the resin matrix. The hydrogen ions generated when the crown ether groups on the resin matrix specifically adsorb lithium can be combined with the amino groups in the resin matrix, thereby further improving the adsorption capacity of the resin for lithium ions; that is, the present invention further improves the adsorption capacity and adsorption selectivity of the resin for lithium ions by utilizing the coordination between the crown ether, the amino group and the specific pore structure in the resin matrix, and is applied to the recovery of lithium elements from the positive electrode material of lithium ion batteries, so that high-purity lithium can be obtained, and the lithium recovery rate is relatively high.
Claims
1. A method for extracting lithium from waste electrolytes, It is characterized in that The steps include: S1: discharging and disassembling the lithium battery to obtain positive electrode waste; adding sodium hydroxide to soak, the liquid-solid ratio of sodium hydroxide to positive electrode waste is 3-10:1, and filtering to obtain positive electrode powder; The active material in the positive electrode waste includes LiCoO 2 、LiNiO 2 、LiMnO 2 One or more of; S2: The positive electrode powder is leached with sulfuric acid having a concentration of 0.3-0.5 mol / L and hydrogen peroxide having a concentration of 30%, and a leachate and a leach residue are obtained after filtering; S3: The leachate is passed through a resin column using an adsorption resin grafted with crown ether as an adsorption medium at a flow rate of 2 BV / h, and the lithium content in the effluent is detected. When the lithium content in the effluent is greater than 0.1 ug / L, the elution is stopped, and the resin column is in an adsorption saturation state; The adsorption resin grafted with crown ether is prepared by the following method: The resin precursor is prepared by suspension polymerization using glycidyl methacrylate, triallyl isocyanurate, azobisisobutyronitrile and n-heptane as the oil phase and water and polyvinyl alcohol as the aqueous phase, with the mass ratio of the aqueous phase to the oil phase being 3:1; the resin precursor is added to a mixed solution of 2-hydroxymethyl-12-crown-4 and sodium hydride, refluxed under a nitrogen atmosphere, and dried to obtain a crown-etherified adsorption resin; the crown-etherified adsorption resin is subjected to epoxy ring opening with ethylenediamine, filtered, washed, and dried to obtain the adsorption resin grafted with the crown ether; S4: Desorbing the resin with dilute hydrochloric acid to obtain a lithium-containing solution.
2. A method for extracting lithium from waste electrolyte according to claim 1, It is characterized in that In step S1, the liquid-to-solid ratio of sodium hydroxide to positive electrode waste is 10:
1.
3. A method for extracting lithium from waste electrolyte according to claim 1, It is characterized in that The specific conditions of step S2 are: adding the positive electrode powder obtained in step S1 to a dilute sulfuric acid solution with a concentration of 0.3-0.5 mol / L at a liquid-solid ratio of 20 mL-30 mL: 1 g to extract lithium, wherein 1 mL of 30% hydrogen peroxide is added to the dilute sulfuric acid solution; leaching at 55-65° C. for 120-200 min, adjusting the pH value of the system to 8.5, filtering, and obtaining a leachate and a leach residue.
4. A method for extracting lithium from waste electrolyte according to claim 1, It is characterized in that In step S3, the rotation speed of the suspension polymerization is 260 r / min, the mass ratio of glycidyl methacrylate to triallyl isocyanurate in the oil phase is 5:1, and the mass ratio of n-heptane to glycidyl methacrylate is 1:
3.
5. A method for extracting lithium from waste electrolyte according to claim 1, It is characterized in that In step S3, the heating rate of the suspension polymerization is: after stirring until the particle size is uniform, the temperature is raised to 85° C. at a rate of 2° C. / min and kept at this temperature for 4 hours.
6. A method for extracting lithium from waste electrolyte according to claim 1, It is characterized in that The crown-etherified adsorption resin described in step S3 is prepared by the following method: 2-Hydroxymethyl-12-crown-4 and sodium hydride were mixed in a molar ratio of 1:1 to obtain a mixed solution, which was stirred at 55°C for 6 hours under a nitrogen atmosphere. A resin precursor was added to the mixed solution, and the mass ratio of the resin precursor to 2-hydroxymethyl-12-crown-4 was 6:
1. The mixture was refluxed for 70 hours under nitrogen protection, filtered, washed, and dried to obtain a crown-etherified adsorption resin.
7. A method for extracting lithium from waste electrolyte according to claim 1, It is characterized in that The specific process conditions for using ethylenediamine to open the epoxy ring in step S3 are: Take the crown etherified adsorption resin, soak it in DMF, and after fully swelling for 24 hours, add ethylenediamine in a mass ratio of 1:5 of crown etherified resin: ethylenediamine, and react at 70°C for 5 hours; after the reaction is completed, cool, filter, wash, and dry to obtain the adsorption resin grafted with crown ether.
8. A method for extracting lithium from waste electrolyte according to claim 1, It is characterized in that The specific process of step S4 is: after disassembling the resin column after adsorption saturation in step S3, immersing it in 1 mol / L dilute hydrochloric acid, the solid-liquid ratio of resin to dilute hydrochloric acid is 1:36-40, and shaking and stirring at 25° C. for 4-6 hours to obtain a lithium-containing solution.
9. A method for extracting lithium from waste electrolyte according to claim 8, It is characterized in that The solid-liquid ratio of resin to dilute hydrochloric acid was 1:36, and the mixture was shaken and stirred at 25°C for 6 hours.
10. A method for extracting and recycling lithium from waste electrolytes, It is characterized in that Add carbonate to the lithium-containing solution obtained by the method according to any one of claims 1 to 9 to obtain battery-grade lithium carbonate.
Citation Information
Patent Citations
Method for separating and recovering lithium from waste lithium ion battery
CN103035977A
Method for recovering and preparing lithium carbonate from positive electrode material of waste lithium ion battery
CN115747521A
Lithium ion specific adsorbent and preparation method and application thereof
CN118079872A
Crown ether modified resin for selective lithium extraction as well as preparation method and application of crown ether modified resin
CN118162119A
Method for manufacturing positive electrode active material for lithium ion secondary battery
JP2021039933A
Cited By
Method for recycling positive electrode material of waste lithium iron phosphate battery based on organic solvent soaking
CN120657303A
Method for recycling positive electrode material of waste lithium iron phosphate battery based on organic solvent soaking
CN120657303B