Hard alloy binding phase material and preparation method thereof
By preparing CoRe solid solution as the binder phase of WC-Co cemented carbide, the problem of insufficient performance of the binder phase Co at high temperatures is solved, and the performance of cemented carbide in high-temperature environments is improved, making it suitable for a wider range of applications.
Patent Information
- Application Number
- CN202410993581.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-15
AI Technical Summary
The binder phase Co in existing WC-Co cemented carbide has low hardness, poor red hardness, and poor corrosion resistance and friction wear resistance, which limits its application in high-temperature environments. In particular, when machining high-temperature alloys for aerospace applications, the binder phase Co softens, oxidizes, and burns, leading to rapid tool failure.
CoRe solid solution was used as the binder phase of a novel high-melting-point cemented carbide. CoRe alloy powder with uniform composition was prepared by vacuum arc furnace alloying, melt spin quenching, and wire electroblasting powder preparation processes. This powder was then used in WC-Co cemented carbide to improve its high-temperature performance.
The prepared CoRe solid solution binder material has a higher melting point, oxidation resistance and red hardness, which improves the bending, compressive and yield strength of WC-Co cemented carbide and makes it suitable for higher temperature applications.
Smart Images

Figure BDA0004959520780000061 
Figure BDA0004959520780000071 
Figure BDA0004959520780000072
Abstract
Description
Technical Field
[0001] The invention belongs to the field of cemented carbide and relates to a novel high melting point cemented carbide bonding phase and a preparation method thereof. Background Art
[0002] WC-Co cemented carbide is widely used in cutting, mineral mining and other fields due to its good comprehensive mechanical properties, and is known as the "teeth of industry". Among them, WC as a hard phase matrix provides WC-Co cemented carbide with good hardness and friction and wear resistance; Co as a bonding phase has excellent wettability with the WC hard phase matrix, which not only reduces the sintering temperature of WC-Co cemented carbide, making it easier to densify, but also gives WC-Co cemented carbide good fracture toughness and bending strength.
[0003] However, the addition of the binder phase Co is also a double-edged sword. Compared with the hard matrix phase, it has lower hardness, poor red hardness, poor corrosion resistance, and poor friction and wear performance, which limits the application of WC-Co cemented carbide. Especially when processing difficult-to-process materials, such as the high-temperature alloy Inconel 718 for aerospace, the temperature between the tool and the cut material is as high as about 1000°C, and the binder phase Co softens, oxidizes, and burns, causing the tool to fail quickly and have a short life. Therefore, it is of great significance to develop a new high-melting point binder phase to improve the high-temperature performance of WC-based cemented carbide.
[0004] The Co binder phase in WC-Co cemented carbide tends to form solid solutions with certain elements over a range of compositions, which provides a way to adjust the properties of WC-Co cemented carbide according to specific needs. Figure 1 ) It can be seen that metal Re can form a continuous solid solution with Co without forming an intermediate phase, and the melting point of the CoRe solid solution can be regulated by regulating the Re content, thereby improving its high temperature performance. Furthermore, after Re is dissolved into the Co lattice, it can cause lattice distortion of Co, increase its deformation resistance, and improve its mechanical properties. Therefore, the CoRe solid solution has a higher melting point, hardness, better oxidation resistance, and better toughness. As a bonding phase, it can improve the bending, compression and yield strength of WC-Co cemented carbide, while giving it better high temperature performance.
[0005] At present, there are few reports on alloying Co and Re to form a solid solution and then using them as a binder phase. Most studies on the enhancement of the binder phase focus on adding Co and Re elements to the WC matrix at the same time. However, since the content of the binder phase is relatively small compared to the WC matrix phase, if the Co and Re elements are not added in the form of a solid solution, they will be separated by the WC matrix, so that a solid solution phase with uniform composition cannot be fully formed, and element aggregation may occur, and the enhancement effect cannot be fully achieved. At the same time, the traditional mechanical alloying method of Co powder and Re powder will not only introduce impurities due to repeated friction and collision between the powder and the grinding ball, but also is not suitable for alloying powders with good plasticity such as Co. The reason is that if the energy is too high, the powder will be cold welded on the surface of the grinding ball and the inner wall of the ball mill, and the particle size will increase. If the energy is insufficient, the solid solution effect will be poor and the distribution of Co and Re elements will be uneven. If the atomization method or rotating electrode powder is used, the powder particle size is too large and the fine powder rate is low. In summary, it is urgent to develop a new preparation process for the new high melting point cemented carbide binder phase. Summary of the invention
[0006] Technical issues
[0007] In order to make up for the deficiencies of the above-mentioned prior art, the present invention aims to provide a new type of high melting point cemented carbide bonding phase material and a preparation method thereof, wherein the cemented carbide bonding phase material has a higher melting point, better oxidation resistance and high temperature properties such as red hardness, and can be used as a bonding phase for high-performance cemented carbide.
[0008] Technical Solution
[0009] According to a first aspect of the present invention, a cemented carbide binder phase material is provided, which is a CoRe solid solution, based on 100wt.% of the total weight of the cemented carbide binder phase material, wherein the Co content is greater than 50wt.% and less than 100wt.%, preferably greater than 60.0wt.% and less than 90.0wt.%; the Re content is greater than 0wt.% and less than or equal to 50wt.%, preferably greater than 10.0wt.% and less than 40.0wt.%.
[0010] Preferably, the melting point of the adhesive phase is 1500°C to 2000°C, more preferably 1600°C to 1900°C.
[0011] Preferably, the average particle size of the cemented carbide binder phase material is less than 60 μm.
[0012] According to a second aspect of the present invention, there is provided a method for preparing the cemented carbide binder phase material of the present invention, comprising the following steps:
[0013] 1) Raw material processing and proportioning: Co block and Re block are respectively subjected to mechanical grinding, degreasing, ultrasonic vibration to remove impurities on the surface of the raw materials and dried, and then the raw materials are proportioned according to the composition;
[0014] 2) Alloying and smelting: placing the processed raw material obtained in step 1) in a vacuum arc furnace, and after gas washing, smelting and alloying for multiple times in an argon atmosphere to obtain a CoRe alloy block with uniform composition;
[0015] 3) Strip spinning: The CoRe alloy block obtained in step 2) is placed in a high vacuum arc melting and crushing system, and after gas washing, the strip is spun by melt spinning method in an argon atmosphere to obtain a CoRe alloy strip;
[0016] 4) Wire electric explosion powder making: Place the CoRe alloy strip in step 3) in the wire electric explosion equipment, adjust the wire feeding position, and close the cavity; fill with argon gas after vacuuming; adjust the charging voltage, and after the voltage display number stabilizes, press the detonation button to explode the strip to prepare powder; after the electric explosion is completed, adjust the voltage display number to zero, and after the discharge rod finishes discharging, collect the powder.
[0017] Preferably, the purity of the Co bulk is 99.9% or more.
[0018] Preferably, the purity of the Re block is 99.9% or more.
[0019] Preferably, step 2) is implemented as follows:
[0020] The vacuum arc melting furnace was evacuated to 3 × 10 -3 Pa, and then introduce argon to 0.04MPa~0.06MPa, and repeat 3 times or more; after washing, check whether there is oxygen through the Ti ingot in the melting furnace and / or remove the oxygen in the furnace; then melt the Co block and Re block 4 times or more to make the Co element and the Re element fully dissolved to form a uniform CoRe alloy solid solution block.
[0021] Preferably, step 3) is implemented as follows:
[0022] The high vacuum arc melting and crushing system was evacuated to 3×10 -3 Pa, and then introduce argon to 0.04MPa~0.06MPa, and repeat 3 times or more; after washing, use induction heating to melt the CoRe alloy block in step 2), and use melt spinning to prepare the molten alloy into a strip, wherein the induced current is slowly increased to 30~50A; the pressure of the molten alloy liquid sprayed onto the water-cooled copper roller is 0.11MPa~0.15MPa; the distance from the nozzle to the water-cooled copper roller is 0.5~10mm; the rotation speed of the water-cooled copper roller is 1500r / min~3000r / min.
[0023] Preferably, the CoRe alloy strip has a thickness of less than 100 μm, a width of less than 3 mm, and a length of more than 150 mm.
[0024] The CoRe alloy strip has uniform composition and structure, and is free of segregation and other impurities.
[0025] Preferably, in step 4), the wire electric explosion chamber is vacuumed to less than 500Pa, filled with argon gas to 1000Pa, the charging voltage is adjusted to 5kV to 20kV, and after the voltage display number is stable, the detonation button is pressed and the electric explosion equipment works.
[0026] According to a third aspect of the present invention, there is provided a WC-CoRe cemented carbide, wherein the binder phase is the binder phase material according to the present invention, and WC serves as a hard phase matrix.
[0027] Preferably, relative to 100wt.% of WC-CoRe cemented carbide, the content of cemented carbide binder phase material is greater than 0wt.% and is less than 25wt.%, preferably 5wt.% to 20wt.%, and the balance is WC.
[0028] According to a fourth aspect of the present invention, there is provided a method for preparing a WC-CoRe cemented carbide according to the present invention, comprising the following steps:
[0029] S1) ball milling the WC powder and the cemented carbide binder phase material prepared according to the present invention in a ball mill and drying;
[0030] S2) placing the dried mixed powder obtained in step S1) into a graphite mold and pre-pressing it at 10 MPa to 20 MPa;
[0031] S3) placing the assembled graphite mold in a spark plasma sintering system, setting the axial pressure to 20MPa-40MPa, the sintering temperature to 1200°C-1600°C, and ending the sintering after keeping the temperature for 0min-10min, and cooling with the furnace.
[0032] The present invention has the following beneficial effects:
[0033] According to the present invention, a method for preparing a cemented carbide binder phase is to alloy commercial Co and Re blocks as raw materials, and then use the melt spinning method to perform belt spinning and wire electric explosion powder making. The production process of this method is environmentally friendly, and the prepared binder phase powder has uniform composition, high purity, high sphericity, no satellite powder or shell powder, good fluidity and not easy to agglomerate, and the melting point can be customized. And the prepared binder phase material has excellent high-temperature properties such as red hardness and high-temperature oxidation resistance, and has good wettability with the cemented carbide matrix, which is very suitable for use as a binder phase of high-performance cemented carbide. Furthermore, the cemented carbide material prepared using the binder phase described in the present invention has better high-temperature performance and is suitable for use in higher temperature occasions. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the phase diagram of Co-Re alloy.
[0035] Figure 2 This is a SEM photograph of the cemented carbide binder phase powder prepared according to Example 1.
[0036] Figure 3 The energy spectrum detection result of the cemented carbide binder phase powder prepared according to Example 1 is shown in FIG.
[0037] Figure 4a and Figure 4b The following are SEM photos showing the microstructure of the WC-CoRe cemented carbide bulk material prepared according to Example 3.
[0038] Figure 5 This is a graph showing the hardness and fracture toughness of samples prepared by directly adding Co powder and Re powder in Comparative Example 1 and adding only Co as a WC cemented carbide binder phase in Comparative Example 2.
[0039] Figure 6 The SEM photograph shows the microstructure of the sample prepared by directly adding Co powder and Re powder as the WC cemented carbide binder phase in Comparative Example 1. DETAILED DESCRIPTION
[0040] The present invention is further described below by way of examples, but the embodiments of the present invention are not limited thereto.
[0041] The vacuum arc melting furnace used in the following examples is from the WK series non-consumable vacuum arc melting furnace of Wuke Optoelectronics (Beijing), China; the belt throwing equipment is from the DXL-500 high vacuum arc melting and crushing system of Shenyang Scientific Instrument Co., Ltd.; the wire electric explosion equipment is a continuous wire electric explosion equipment for preparing micro-nano powders; the cemented carbide sintering equipment is from SINTER LAND Co., Ltd., Japan, and the model is LABOX series. It should be noted that the preparation of a new high melting point cemented carbide binder phase using the method of the present invention and equipment of other manufacturers and models is also within the scope of the present invention.
[0042] Used in the following examples:
[0043] Co blocks were commercially available with a purity of 99.9%.
[0044] Re blocks were commercially available with a purity of 99.9%.
[0045] The WC powder was commercially available with a purity of 99.9% and a particle size of 0.2 μm to 1 μm.
[0046] Figure 1 is the Co-Re alloy phase diagram, Figure 1 It can be seen that metallic Re can form a continuous solid solution with Co without forming an intermediate phase, and the melting point of the CoRe solid solution can be regulated by adjusting the Re content.
[0047] Example 1
[0048] The novel high melting point cemented carbide binder phase was prepared according to the following steps:
[0049] 1) Raw material processing and proportioning: The commercially available Co block and Re block were sanded, ultrasonically cleaned, and dried, and 21.25 g of Co block and 3.75 g of Re block were weighed respectively, wherein the content of Re was 15 wt.%;
[0050] 2) Alloying and melting: Place the raw materials in step 1) in a vacuum arc furnace, and evacuate the vacuum arc melting furnace to 3×10 -3 Pa, high purity argon is introduced to 0.05MPa, and repeated 3 times. After gas washing, the Ti ingot in the melting furnace is used to check the presence of oxygen and / or further remove oxygen. Then the Co and Re blocks are repeatedly turned over and melted 4 times to obtain a CoRe alloy solid solution block;
[0051] 3) Belt throwing: Place the CoRe alloy solid solution block in step 2) in a high vacuum arc melting and crushing system, adjust the distance from the nozzle to the water-cooled copper roller to 10 mm; vacuum is drawn to 3×10 -3 Pa, and then introduce high-purity argon to 0.05MPa, and repeat 3 times. Adjust the rotation speed of the water-cooled copper roller to 2000r / min, then slowly increase the induced current to 40A, use induction heating to melt the CoRe alloy block in step 2), set the pressure of the molten alloy sprayed onto the water-cooled copper roller to 0.13MPa, and spray the molten alloy onto the rotating water-cooled copper roller through the nozzle. The prepared CoRe alloy strip has a thickness of less than 100μm, a width of less than 3mm, a length of more than 150mm, uniform composition and structure, and no segregation and other impurities;
[0052] 4) Wire electric explosion powder making: Place the CoRe alloy strip in step 3) in the wire electric explosion equipment, evacuate the chamber to 500Pa, fill it with high-purity argon gas to 1000Pa, and adjust the charging voltage to 11kV. After the voltage display is stable, press the detonation button, and the strip explodes to prepare powder. After the electric explosion is over, adjust the voltage display to zero, and after the discharge rod is discharged, collect the powder to obtain CoRe alloy powder;
[0053] The specific parameters are shown in Table 1.
[0054] Table 1: Relevant properties of the new high melting point cemented carbide binder phase prepared in Example 1
[0055]
[0056] Figure 2 is a SEM photograph of the new high melting point cemented carbide binder phase powder prepared according to Example 1. Figure 2 It can be seen that the powder particles have high sphericity and no satellite powder or shell-shaped powder.
[0057] Figure 3 The energy spectrum test results of the new high melting point cemented carbide binder phase powder prepared according to Example 1 are as follows: Figure 3 It can be seen that Co and Re elements are fully dissolved in solid without segregation enrichment and other impurities.
[0058] Example 2
[0059] The novel high melting point cemented carbide binder phase was prepared according to the following steps:
[0060] 1) Raw material processing and proportioning: The commercially available Co block and Re block were sanded, ultrasonically cleaned, and dried, and 22.50 g of Co block and 2.50 g of Re block were weighed respectively, wherein the content of Re was 10 wt.%;
[0061] 2) Alloying and melting: Place the raw materials in step 1) in a vacuum arc furnace, and evacuate the vacuum arc melting furnace to 3×10 -3 Pa, high purity argon is introduced to 0.05MPa, and repeated 3 times. After gas washing, the Ti ingot in the melting furnace is used to check the presence of oxygen and / or further remove oxygen. Then the Co and Re blocks are repeatedly turned over and melted 4 times to obtain a CoRe alloy solid solution block;
[0062] 3) Belt throwing: Place the CoRe alloy solid solution block in step 2) in a high vacuum arc melting and crushing system, adjust the distance from the nozzle to the water-cooled copper roller to 10 mm; vacuum is drawn to 3×10 -3 Pa, and then high-purity argon is introduced to 0.05MPa, and repeated 3 times. The rotation speed of the water-cooled copper roller is adjusted to 2000r / min, and then the induced current is slowly increased to 40A, and the CoRe alloy block in step 2) is melted by induction heating, and the pressure of the molten alloy sprayed onto the water-cooled copper roller is set to 0.13MPa, and the molten alloy is sprayed onto the rotating water-cooled copper roller through a nozzle. The prepared CoRe alloy strip has a thickness of less than 100μm, a width of less than 3mm, and a length of more than 150mm, with uniform composition and structure, and no segregation and other impurities;
[0063] 4) Wire electric explosion powder making: Place the CoRe alloy strip in step 3) in the wire electric explosion equipment, evacuate the chamber and fill it with high-purity argon gas to 1000Pa, and adjust the charging voltage to 11kV. After the voltage display is stable, press the detonation button, and the strip explodes to prepare powder. After the electric explosion is over, adjust the voltage display to zero, and after the discharge rod is discharged, collect the powder to obtain CoRe alloy powder;
[0064] The specific parameters are shown in Table 2.
[0065] Table 2: Relevant properties of the new high melting point cemented carbide binder phase prepared in Example 2
[0066]
[0067] Example 3
[0068] A novel high melting point bonding phase WC cemented carbide bulk material is prepared according to the following steps, wherein the weight ratio of WC powder to Co-15Re alloy powder is 9:1.
[0069] 1) Powder mixing: WC powder and Co-15Re cemented carbide material powder prepared in Example 1 are weighed according to the above weight ratio, and the weighed powders are put into a ball mill for ball milling. The ball milled powders are dried.
[0070] 2) Mold filling: The mixed powder obtained after drying in step 1) is placed in a graphite mold and pre-pressed at 20 MPa.
[0071] 3) Sintering: Place the assembled graphite mold in a spark plasma sintering system, set the axial pressure to 40 MPa, the sintering temperature to 1320°C, and end the sintering after keeping warm for 3 minutes, and cool with the furnace.
[0072] 4) Sampling and testing: Take out the samples, cut, grind and polish them, and test the performance. The specific performance parameters are shown in Table 3.
[0073] Table 3: Properties of the new high melting point binder phase WC cemented carbide block material prepared in Example 3
[0074]
[0075] Comparative Example 1
[0076] Reference 1: "WC-Co-Re cemented carbides: Structure, properties and potential applications" (International Journal of Refractory Metals and Hard Materials, Volume 78, 2019, Pages 247-253, ISSN 0263-4368) reported that the hardness and fracture toughness of samples prepared by directly adding Co powder and Re powder as the WC cemented carbide binder phase are as follows: Figure 5 As shown by the red dots in the middle, the horizontal axis is the Vickers hardness value of the material, and the vertical axis is the fracture toughness value of the material; its microscopic morphology is as follows Figure 6 shown.
[0077] It can be seen that the hardness of the sample prepared by directly adding Co powder and Re powder as the binder phase of WC cemented carbide is about 1600HV30 and the fracture toughness is about 10MPa·m 1 / 2 , there is an abnormal aggregation distribution of Re; since the Co and Re elements are not alloyed and the whole is used as a bonding phase, Re may not be fully dissolved into the Co lattice, thereby failing to fully strengthen the bonding phase, and may also lead to uneven bonding phase composition. All of the above will affect the performance of the final prepared cemented carbide.
[0078] Comparative Example 2
[0079] Reference 2: Hardmetals-microstructural design, testing and property maps (Proceedings of the 15th International Plansee Seminar, vol. 4, Plansee Group Reutte, Austria, 2001, pp. 245-266.) reported that the hardness and fracture toughness of the samples prepared by adding only Co as the binder phase of WC cemented carbide are as follows: Figure 5 As shown. The black dot curve represents the combined baseline of Vickers hardness and fracture toughness of WC-Co cemented carbide material when the addition amount of Co binder phase is 6wt.%; the triangle curve represents the combined baseline of Vickers hardness and fracture toughness of WC-Co cemented carbide material when the addition amount of Co binder phase is 10wt.%; the square curve represents the combined baseline of Vickers hardness and fracture toughness of WC-Co cemented carbide material when the addition amount of Co binder phase is 15wt.%.
[0080] It can be seen that: compared with Example 3 of the present invention, the performance of the cemented carbide material prepared by using CoRe alloy as the binder phase is equivalent to that of the conventional cemented carbide material prepared by using Co as the binder phase, and, as the results reported in Comparative Example 1: the addition of the high-temperature element Re can improve the high-temperature performance of WC cemented carbide and broaden its application field. Therefore, the present invention has important application value and practical application prospects.
[0081] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A cemented carbide binder phase material, which is a CoRe solid solution, based on 100wt.% of the total weight of the cemented carbide binder phase material, in, The content of Co is greater than 50 wt.% and less than 100 wt.%, preferably greater than 60.0 wt.% and less than 90.0 wt.%; the content of Re is greater than 0 wt.% and less than or equal to 50 wt.%, preferably greater than 10.0 wt.% and less than 40.0 wt.%.
2. The cemented carbide binder phase material according to claim 1, in, The melting point of the cemented carbide binder phase material is 1500°C to 2000°C, preferably 1600°C to 1900°C; and / or The average particle size of the cemented carbide binder phase material is less than 60 μm.
3. A method for preparing the cemented carbide binder phase material according to claim 1 or 2, comprising the following steps: 1) Raw material processing and proportioning: Co block and Re block are respectively subjected to mechanical grinding, degreasing, ultrasonic vibration to remove impurities on the surface of the raw materials and dried, and then the raw materials are proportioned according to the composition; 2) Alloying and smelting: placing the processed raw material obtained in step 1) in a vacuum arc furnace, and after gas washing, smelting and alloying for multiple times in an argon atmosphere to obtain a CoRe alloy block with uniform composition; 3) Strip spinning: The CoRe alloy block obtained in step 2) is placed in a high vacuum arc melting and crushing system, and after gas washing, the strip is spun by melt spinning method in an argon atmosphere to obtain a CoRe alloy strip; 4) Wire electric explosion powder making: Place the CoRe alloy strip in step 3) in the wire electric explosion equipment, adjust the wire feeding position, and close the cavity; fill with argon gas after vacuuming; adjust the charging voltage, and after the voltage display number stabilizes, press the detonation button to explode the strip to prepare powder; after the electric explosion is completed, adjust the voltage display number to zero, and after the discharge rod finishes discharging, collect the powder.
4. The method for preparing a cemented carbide binder phase material according to claim 3, in, The purity of Co block is 99.9% or more; and / or The purity of Re block is 99.9% or more.
5. The method for preparing a cemented carbide binder phase material according to claim 3 or 4, in, Step 2) is implemented as follows: The vacuum arc melting furnace was evacuated to 3 × 10 -3 Pa, then introduce argon gas to 0.04MPa-0.06MPa, repeat 3 times or more; after gas washing, check whether there is oxygen through the Ti ingot in the melting furnace and / or remove the oxygen in the furnace; then melt the Co block and Re block 4 times or more to make the Co element and the Re element fully dissolved to form a uniform CoRe alloy solid solution block; and / or Step 3) is implemented as follows: The high vacuum arc melting and crushing system was evacuated to 3×10 -3 Pa, and then introduce argon to 0.04MPa~0.06MPa, and repeat 3 times or more; after washing, use induction heating to melt the CoRe alloy block in step 2), and use melt spinning to prepare the molten alloy into a strip, wherein the induced current is slowly increased to 30A~50A; the pressure of the molten alloy liquid sprayed onto the water-cooled copper roller is 0.11MPa~0.15MPa; the distance from the nozzle to the water-cooled copper roller is 0.5mm~10mm; the rotation speed of the water-cooled copper roller is 1500r / min~3000r / min.
6. The method for preparing a cemented carbide binder phase material according to any one of claims 3 to 5, in, The CoRe alloy strip has a thickness of less than 100 μm, a width of less than 3 mm, and a length of more than 150 mm; and / or In step 4), the wire electric explosion chamber is evacuated to less than 500Pa, filled with argon gas to 1000Pa, and the charging voltage is adjusted to 5kV to 20kV. After the voltage display is stable, the detonation button is pressed and the electric explosion equipment starts working.
7. A WC-CoRe cemented carbide comprising the cemented carbide binder phase material according to claim 1 or 2.
8. The WC-CoRe cemented carbide according to claim 8, in, Relative to 100wt.% of WC-CoRe cemented carbide, wherein the cemented carbide contains more than 0wt.% and less than 25wt.% of the cemented carbide binder phase material, and the balance is WC.
9. The WC-CoRe cemented carbide according to claim 8, in, The cemented carbide contains 5wt.% to 20wt.% of the cemented carbide binder phase material, and the remainder is WC.
10. A method for preparing a WC-CoRe cemented carbide according to any one of 7 to 9, comprising the following steps: S1) milling WC powder and the cemented carbide binder phase material according to claim 1 or 2 in a ball mill and drying; S2) placing the dried mixed powder obtained in step S1) into a graphite mold and pre-pressing it at 10 MPa to 20 MPa; S3) placing the assembled graphite mold in a spark plasma sintering system, setting the axial pressure to 20MPa-40MPa, the sintering temperature to 1200°C-1600°C, and ending the sintering after keeping the temperature for 0min-10min, and cooling with the furnace.