Nickel-based corrosion-resistant alloy and preparation method thereof

By optimizing the composition and preparation process of nickel-based alloy, Ce, Er and Hf are added to form a dual protective layer, the problem of insufficient corrosion resistance of nickel-based alloys in extreme corrosion environments is solved, and its corrosion resistance and equipment use are significantly improved. life.

CN118957363APending Publication Date: 2024-11-15QINHUANGDAO HECHENG NICKEL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411145488.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In extreme corrosion environments, traditional nickel-based alloys have insufficient corrosion resistance, such as strong acid and alkali media, water vapor environments under high temperature and high pressure, and marine environments rich in salt and microorganisms, which are difficult to meet the high requirements of modern industry for material performance.

Method used

By optimizing the composition of the nickel-based alloy, adding Ce, Er and Hf, synergistically strengthening the alloy, we prepare hafnium boronide solid blocks and corrosion-resistant coatings, using ball milling, sintering, smelting, forging and spraying processes to form a double protective layer to enhance corrosion resistance to performance.

Benefits of technology

The corrosion resistance of nickel-based alloys is significantly improved. By refining grains and forming protective films, it effectively blocks the penetration of corrosive media, extends the service life of the equipment and reduces maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides a nickel-based corrosion-resistant alloy and a preparation method thereof, and belongs to the technical field of alloy preparation. The preparation process comprises the following steps: preparing hafnium boride solid blocks; preparing a nickel-based alloy; preparing a corrosion-resistant coating; and preparing the nickel-based corrosion-resistant alloy. By optimizing alloy components and adding Ce, Er and Hf, Ce, Er and Hf synergistically strengthen the nickel-based alloy to enable precipitated phases to be distributed intermittently along a grain boundary, coarsening of a grain boundary precipitation-free precipitation zone is inhibited, meanwhile, particles are dispersed, particle clusters are reduced, grains are refined, a fine grain structure can provide more grain boundaries, and under the combined action of Ce, Er and Hf, the grain boundaries can provide more grain boundaries, so that the grain boundaries have a better grain separation effect. And the double protection layers not only enhance the original oxidation resistance, but also effectively obstruct the corrosive medium, so that the corrosion resistance of the nickel-based alloy is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy preparation, and in particular to a nickel-based corrosion-resistant alloy and a preparation method thereof. Background Art

[0002] In the current era of rapid development of global industry, especially in cutting-edge fields such as energy conversion, chemical production, aerospace exploration and marine resource development, the performance of materials is directly related to the operating efficiency, safety and long-term economy of facilities. Among them, corrosion resistance and comprehensive mechanical properties are the two core indicators for evaluating whether materials can adapt to extreme operating environments. These fields often face severe tests such as extreme temperature fluctuations, high-pressure environments, and highly corrosive media, which put forward unprecedented high requirements on the durability and reliability of materials.

[0003] Nickel-based alloys, as a type of high-performance material, have long played an important role in these demanding applications due to their excellent high temperature resistance, excellent corrosion resistance and good mechanical strength. For example, in high-temperature gas turbine blades, petroleum refining equipment, deep-sea drilling facilities and spacecraft thermal protection systems, the use of nickel-based alloys has greatly improved the stability and service life of the equipment, reduced maintenance costs and ensured operational safety.

[0004] However, technological progress and industrial upgrading have put forward higher expectations for material performance. Although traditional nickel-based alloys perform well under most harsh conditions, their corrosion resistance still faces severe challenges in certain extreme corrosive environments, such as long-term exposure to strong acid and alkali media, water vapor environments under high temperature and high pressure, and marine environments rich in salt and microorganisms.

[0005] Therefore, we proposed a nickel-based corrosion-resistant alloy and a preparation method thereof which can improve the corrosion resistance of the alloy. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention aims to provide a nickel-based corrosion-resistant alloy and a preparation method thereof.

[0007] A nickel-based corrosion-resistant alloy, wherein the nickel-based alloy comprises the following components: C≤0.005wt%, 0.04-0.08wt%Si, 0.3-0.8wt%Mn, 14.5-16.5wt%Cr, 15-17wt%Mo, 3.0-4.5wt%W, 4-7wt%Fe, Co≤1.5wt%, 0.1-0.2wt%V, 0.01-0.05wt%Ce, 0.05-0.1wt%Er, 0.05-0.2wt%Hf, 0.003-0.006wt%P, and the balance is Ni and unavoidable impurities.

[0008] Preferably, the nickel-based alloy composition is: C≤0.005wt%, 0.04-0.08wt%Si, 0.3-0.8wt%Mn, 14.5-16.5wt%Cr, 15-17wt%Mo, 3.0-4.5wt%W, 4-7wt%Fe, Co≤1.5wt%, 0.1-0.2wt%V, 0.03-0.04wt%Ce, 0.07-0.09wt%Er, 0.06-0.13wt%Hf, 0.004-0.005wt%P, and the balance is Ni and unavoidable impurities.

[0009] A method for preparing a nickel-based corrosion-resistant alloy comprises the following steps: Step 1: Preparation of solid block of hafnium boride Boric acid and citric acid are mixed and added to hafnium oxide nanopowder, and then ball-milled and sintered to finally obtain a hafnium boride solid block; Step 2: Preparation of mixed powder Firstly, the raw materials except the hafnium boride solid block are melted and refined, and then the hafnium boride solid block is added for further refining to prepare a vacuum ingot, which is then forged, rolled and heat treated to finally obtain a nickel-based alloy.

[0010] Furthermore, step 1 of preparing the hafnium boride solid block specifically comprises the following steps: Step 1.1: dissolving 3-3.5 parts by weight of boric acid and 0.5-0.7 parts by weight of citric acid in 8-10 parts by weight of deionized water, stirring at 80-100° C. for 3-5 hours to obtain a mixed solution; Step 1.2: Add 1-2 parts by weight of hafnium oxide nanopowder to the mixed solution, mix and stir to form a slurry, and place the slurry in a planetary ball mill to obtain a prefabricated slurry; Step 1.3: The prefabricated slurry is first dried and then placed in a tubular furnace for sintering. The temperature is increased and then kept warm under vacuum to finally obtain a solid block of hafnium boride.

[0011] Furthermore, the preparation of the nickel-based alloy in step 2 specifically comprises the following steps: Step 2.1: The nickel-based alloy composition is: C≤0.005wt%, 0.04-0.08wt%Si, 0.3-0.8wt%Mn, 14.5-16.5wt%Cr, 15-17wt%Mo, 3.0-4.5wt%W, 4-7wt%Fe, Co≤1.5wt%, 0.1-0.2wt%V, 0.01-0.05wt%Ce, 0.05-0.1wt%Er, 0.05-0.2wt%Hf, 0.003-0.006wt%P, and the balance is Ni and unavoidable impurities; Step 2.2: according to the above ratio, take the raw materials except the solid block of hafnium boride for smelting, refine at 1530-1550°C for 20-30min, add the solid block of hafnium boride, continue to keep warm and stir for 20-30min, and the casting temperature is 1510-1530°C; Step 2.3: The vacuum ingot is subjected to electroslag remelting, forging, rolling, and heat treatment to finally obtain a nickel-based alloy.

[0012] Furthermore, the specific parameters of heat preservation after heating under vacuum state in step 1.3 are heating to 650-700°C and maintaining for 0.5-1h, then heating to 1100-1150°C and maintaining for 1-2h, and then heating again to 1550-1600°C and maintaining for 2-3h.

[0013] Furthermore, the smelting time in step 2.2 is 1 to 2 hours.

[0014] Furthermore, the method further comprises spraying a corrosion-resistant coating on the nickel-based alloy, comprising the following steps: Step I: Preparation of corrosion-resistant coating The corrosion-resistant coating is prepared by using an organic resin binder, a corrosion inhibitor, a lubricant and a mixed solvent; Step II: Preparation of nickel-based corrosion-resistant alloy The prepared corrosion-resistant coating is sprayed evenly on the rough surface of the nickel-based alloy by a spraying process, and the nickel-based corrosion-resistant alloy is obtained after curing.

[0015] Furthermore, the preparation of the corrosion-resistant coating in step I specifically comprises the following steps: Step I.I: dissolving 20-30 parts by weight of novolac epoxy resin and 10-20 parts by weight of phenolic resin in 50-80 parts by weight of a mixed solvent, stirring evenly to obtain a solution I, wherein the mixed solvent is ethylene glycol ethyl ether, butanone and toluene in a volume ratio of 5:3:10; Step I.II: grind and disperse 30-50 parts by weight of polytetrafluoroethylene powder through a cone mill, add it to 30-50 parts by weight of a mixed solvent, mix well, add 2-4 parts by weight of 2-(1,3-benzothiazole-2-thio)succinic acid, stir and disperse at 300-500 r / min for 10-20 minutes, and obtain solution II; Step I.III: Mix solution I and solution II and mix them evenly with a high-speed stirrer to obtain a corrosion-resistant coating.

[0016] Furthermore, step II of preparing the nickel-based corrosion-resistant alloy specifically comprises the following steps: Step II.I: After removing grease, scale, pollutants, etc. from the surface of the nickel-based alloy, mechanical grinding is performed for 20-30 seconds to obtain a nickel-based alloy with a rough surface; Step II.II: The coating is evenly sprayed on the rough surface of the nickel-based alloy by a spraying process, and the coating is solidified after being dried to obtain a nickel-based corrosion-resistant alloy.

[0017] Furthermore, the curing conditions in step II.II are: curing at 190-195°C for 1.5-2h.

[0018] The working principle and beneficial effects of the present invention are: 1. The present invention optimizes the alloy composition, adds Ce, Er and Hf, and the three synergistically strengthen the nickel-based alloy so that the precipitation phase is discontinuously distributed along the grain boundary, inhibits the coarsening of the non-precipitation zone at the grain boundary, and disperses the particles, reduces particle clusters, and refines the grains. The fine grain structure can provide more grain boundaries to block further penetration of corrosive media. This double protective layer not only enhances the original antioxidant ability, but also effectively blocks the corrosive medium, thereby improving the corrosion resistance of the nickel-based alloy.

[0019] 2. The present invention prepares a corrosion-resistant coating using an organic resin binder, a corrosion inhibitor, a lubricant and a mixed solvent, thereby achieving a second level of protection against corrosion of nickel-based alloys. By adding 2-(1,3-benzothiazole-2-thio)succinic acid as a corrosion inhibitor, the concept of active chemical corrosion inhibition protection is combined with the concept of passive physical barrier defense. The active groups in the molecular structure of 2-(1,3-benzothiazole-2-thio)succinic acid can be well adsorbed on the surface of the substrate to form a protective film, and 2-(1,3-benzothiazole-2-thio)succinic acid can react with the corroded substrate surface to generate a complex that accumulates on the substrate surface to form a passivation film, thereby preventing the penetration of corrosive media, thereby effectively improving the corrosion resistance of the coating.

[0020] 3. The present invention introduces lubricant polytetrafluoroethylene into the corrosion-resistant coating. Polytetrafluoroethylene can transform the coating from hydrophilic to hydrophobic, further improving the shielding and barrier properties of the coating and enhancing the corrosion resistance of the coating. DETAILED DESCRIPTION

[0021] The following is a detailed description of a method for preparing a nickel-based corrosion-resistant alloy provided by the present invention in conjunction with specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternative methods to implement some known technologies.

[0022] Example 1 A method for preparing a nickel-based corrosion-resistant alloy comprises the following steps: Step 1: Preparation of solid block of hafnium boride Step 1.1: dissolving 3 parts by weight of boric acid and 0.5 parts by weight of citric acid in 8 parts by weight of deionized water, stirring at 80° C. for 3 hours to obtain a mixed solution; Step 1.2: Add 1 part by weight of hafnium oxide nanopowder to the mixed solution, mix and stir to form a slurry, and place the slurry in a planetary ball mill to obtain a prefabricated slurry; Step 1.3: The prefabricated slurry is first dried and then sintered in a tubular furnace. The temperature is raised to 650°C in a vacuum state and maintained for 0.5 h, then raised to 1100°C and maintained for 1 h, and then raised to 1550°C and maintained for 2 h, to finally obtain a solid block of hafnium boride; Step 2: Preparation of nickel-based alloy Step 2.1: The nickel-based alloy composition is: 0.005wt%C, 0.04wt%Si, 0.3wt%Mn, 14.5wt%Cr, 15wt%Mo, 3.0wt%W, 4wt%Fe, 1wt%Co, 0.1wt%V, 0.01wt%Ce, 0.05wt%Er, 0.05wt%Hf, 0.003wt%P, and the balance is Ni and unavoidable impurities; Step 2.2: according to the above ratio, the raw materials except the solid block of hafnium boride are melted for 1 hour, refined at 1530°C for 20 minutes, and the solid block of hafnium boride is added, and the heat preservation and stirring treatment is continued for 30 minutes. The casting temperature is 1510°C to obtain a vacuum ingot; Step 2.3: The vacuum ingot is subjected to electroslag remelting, forging, rolling and heat treatment by conventional means to finally obtain a nickel-based alloy.

[0023] Example 2 A method for preparing a nickel-based corrosion-resistant alloy comprises the following steps: Step 1: Preparation of solid block of hafnium boride Step 1.1: dissolving 3 parts by weight of boric acid and 0.5 parts by weight of citric acid in 8 parts by weight of deionized water, stirring at 80° C. for 3 hours to obtain a mixed solution; Step 1.2: Add 1 part by weight of hafnium oxide nanopowder to the mixed solution, mix and stir to form a slurry, and place the slurry in a planetary ball mill to obtain a prefabricated slurry; Step 1.3: The prefabricated slurry is first dried and then sintered in a tubular furnace. The temperature is raised to 650°C in a vacuum state and maintained for 0.5 h, then raised to 1100°C and maintained for 1 h, and then raised to 1550°C and maintained for 2 h, to finally obtain a solid block of hafnium boride; Step 2: Preparation of nickel-based alloy Step 2.1: The nickel-based alloy composition is: 0.005wt%C, 0.04wt%Si, 0.3wt%Mn, 14.5wt%Cr, 15wt%Mo, 3.0wt%W, 4wt%Fe, 1wt%Co, 0.1wt%V, 0.03wt%Ce, 0.07wt%Er, 0.06wt%Hf, 0.004wt%P, and the balance is Ni and unavoidable impurities; Step 2.2: according to the above ratio, the raw materials except the solid block of hafnium boride are smelted for 2 hours, refined at 1550°C for 20 minutes, and the solid block of hafnium boride is added, and the heat preservation and stirring treatment is continued for 25 minutes. The casting temperature is 1530°C to obtain a vacuum ingot; Step 2.3: The vacuum ingot is subjected to electroslag remelting, forging, rolling, and heat treatment to finally obtain a nickel-based alloy.

[0024] Example 3 A method for preparing a nickel-based corrosion-resistant alloy comprises the following steps: Step 1: Preparation of solid block of hafnium boride Step 1.1: dissolving 3 parts by weight of boric acid and 0.5 parts by weight of citric acid in 8 parts by weight of deionized water, stirring at 80° C. for 3 hours to obtain a mixed solution; Step 1.2: Add 1 part by weight of hafnium oxide nanopowder to the mixed solution, mix and stir to form a slurry, and place the slurry in a planetary ball mill to obtain a prefabricated slurry; Step 1.3: The prefabricated slurry is first dried and then sintered in a tubular furnace. The temperature is raised to 650°C in a vacuum state and maintained for 0.5 h, then raised to 1100°C and maintained for 1 h, and then raised to 1550°C and maintained for 2 h, to finally obtain a solid block of hafnium boride; Step 2: Preparation of nickel-based alloy Step 2.1: The nickel-based alloy composition is: 0.003wt%C, 0.04wt%Si, 0.3wt%Mn, 14.5wt%Cr, 15wt%Mo, 3.0wt%W, 4wt%Fe, 1wt%Co, 0.1wt%V, 0.04wt%Ce, 0.09wt%Er, 0.13wt%Hf, 0.005wt%P, and the balance is Ni and unavoidable impurities; Step 2.2: according to the above ratio, the raw materials except the solid block of hafnium boride are smelted for 1 hour, refined at 1540°C for 20 minutes, and the solid block of hafnium boride is added, and the heat preservation and stirring treatment is continued for 25 minutes. The casting temperature is 1520°C to obtain a vacuum ingot; Step 2.3: The vacuum ingot is subjected to electroslag remelting, forging, rolling, and heat treatment to finally obtain a nickel-based alloy.

[0025] Example 4 A method for preparing a nickel-based corrosion-resistant alloy comprises the following steps: Step 1: Preparation of solid block of hafnium boride Step 1.1: dissolving 3.5 parts by weight of boric acid and 0.7 parts by weight of citric acid in 10 parts by weight of deionized water, stirring at 100° C. for 5 hours to obtain a mixed solution; Step 1.2: Add 2 parts by weight of hafnium oxide nanopowder to the mixed solution, mix and stir to form a slurry, and place the slurry in a planetary ball mill to obtain a prefabricated slurry; Step 1.3: The prefabricated slurry is first dried and then sintered in a tubular furnace. The temperature is raised to 700°C in a vacuum state and maintained for 1 hour, then raised to 1150°C and maintained for 2 hours, and then raised to 1600°C and maintained for 3 hours, to finally obtain a solid block of hafnium boride; Step 2: Preparation of nickel-based alloy Step 2.1: The nickel-based alloy composition is: 0.002wt%C, 0.08wt%Si, 0.8wt%Mn, 16.5wt%Cr, 17wt%Mo, 4.5wt%W, 7wt%Fe, 1.5wt%Co, 0.2wt%V, 0.05wt%Ce, 0.1wt%Er, 0.2wt%Hf, 0.006wt%P, and the balance is Ni and unavoidable impurities; Step 2.2: according to the above ratio, the raw materials except the solid block of hafnium boride are smelted for 1 hour, refined at 1550°C for 30 minutes, and the solid block of hafnium boride is added, and the heat preservation and stirring treatment is continued for 30 minutes. The casting temperature is 1510°C to obtain a vacuum ingot; Step 2.3: The vacuum ingot is subjected to electroslag remelting, forging, rolling, and heat treatment to finally obtain a nickel-based alloy.

[0026] Example 5 Based on the same concept as the above-mentioned embodiment 1, on the basis of embodiment 1, this embodiment further includes the following steps: Step I: Preparation of corrosion-resistant coating Step I.I: dissolving 20 parts by weight of novolac epoxy resin and 10 parts by weight of phenolic resin in 50 parts by weight of a mixed solvent, stirring evenly, to obtain a solution I, wherein the mixed solvent is ethylene glycol ethyl ether, butanone and toluene in a volume ratio of 5:3:10; Step I.II: grind and disperse 30 parts by weight of polytetrafluoroethylene powder through a cone mill, add the powder to 30 parts by weight of a mixed solvent, mix well, add 2 parts by weight of 2-(1,3-benzothiazole-2-thio)succinic acid, stir and disperse at 300 r / min for 10 minutes, and obtain solution II; Step I.III: Mix solution I and solution II and mix them evenly with a high-speed stirrer to obtain a corrosion-resistant coating; Step II: Preparation of nickel-based corrosion-resistant alloy Step II.I: removing grease, scale, pollutants, etc. from the surface of the nickel-based alloy by conventional means, and then mechanically polishing for 20 seconds to obtain a nickel-based alloy with a rough surface; Step II.II: The coating is evenly sprayed on the rough surface of the nickel-based alloy by a spraying process. After the coating is surface-dried, it is cured at 190° C. for 1.5 hours to obtain a nickel-based corrosion-resistant alloy.

[0027] Comparative Example 1 Compared with Example 1, the difference of Comparative Example 1 is that the nickel-based alloy composition in Comparative Example 1 is: 0.005wt% C, 0.04wt% Si, 0.3wt% Mn, 14.5wt% Cr, 15wt% Mo, 3.0wt% W, 4wt% Fe, 1wt% Co, 0.1wt% V, 0.11wt% Ce, and the balance is Ni and unavoidable impurities, and the remaining steps are unchanged to prepare the nickel-based alloy, which is recorded as Comparative Example 1.

[0028] Comparative Example 2 Compared with Example 1, the difference of Comparative Example 2 is that the nickel-based alloy composition in Comparative Example 2 is: 0.005wt% C, 0.04wt% Si, 0.3wt% Mn, 14.5wt% Cr, 15wt% Mo, 3.0wt% W, 4wt% Fe, 1wt% Co, 0.1wt% V, 0.11wt% Er, and the balance is Ni and unavoidable impurities, and the remaining steps are unchanged to prepare the nickel-based alloy, which is recorded as Comparative Example 2.

[0029] Comparative Example 3 Compared with Example 1, the difference of Comparative Example 3 is that the nickel-based alloy composition in Comparative Example 3 is: 0.005wt% C, 0.04wt% Si, 0.3wt% Mn, 14.5wt% Cr, 15wt% Mo, 3.0wt% W, 4wt% Fe, 1wt% Co, 0.1wt% V, 0.11wt% Hf, 0.005wt% P, and the balance is Ni and unavoidable impurities. The remaining steps are unchanged to prepare the nickel-based alloy, which is recorded as Comparative Example 3.

[0030] Corrosion resistance: The corrosion rate is taken as the average of three times, and the GB / T 19746-2018 method is used for testing.

[0031] The corrosion resistance of Examples 1-4 and Comparative Examples 1-3 was measured, and the measurement results are shown in Table 1.

[0032] Table 1. Corrosion resistance test results of Examples 1-4 and Comparative Examples 1-3

[0033] It can be seen from the data in Table 1 that the data of Examples 1 and 4 are higher than those of Examples 2-3, indicating that the ratio of 0.03-0.04wt% Ce, 0.07-0.09wt% Er, and 0.06-0.13wt% Hf is optimal. It can be seen from the data of Example 1 and Comparative Examples 1-3 that the simultaneous addition of Ce, Er, and Hf has a significant effect on improving the corrosion resistance of the nickel-based alloy, indicating that the simultaneous addition of the three has a certain synergistic effect and can effectively improve the corrosion resistance of the nickel-based alloy.

[0034] Comparative Example 4 Compared with Example 5, the difference of Comparative Example 4 is that in Comparative Example 4, steps I.II are replaced by "grinding and dispersing 30 parts by weight of polytetrafluoroethylene powder through a conical mill, adding to 30 parts by weight of a mixed solvent, and mixing evenly to obtain a solution II", and the remaining steps remain unchanged to prepare a nickel-based corrosion-resistant alloy, which is recorded as Comparative Example 4.

[0035] Comparative Example 5 Compared with Example 5, the difference of Comparative Example 5 is that in Comparative Example 5, steps I.II are replaced by "adding 2 parts by weight of 2-(1,3-benzothiazole-2-thio)succinic acid to 30 parts by weight of a mixed solvent, stirring and dispersing at 300 r / min for 10 minutes, and mixing evenly to obtain a solution II", and the remaining steps remain unchanged to prepare a nickel-based corrosion-resistant alloy, which is recorded as Comparative Example 5.

[0036] Corrosion resistance: The corrosion rate is taken as the average of three times, and the GB / T 19746-2018 method is used for testing.

[0037] Using the data of Example 1, the corrosion resistance of Example 5 and Comparative Examples 4-5 was measured. The measurement results are shown in Table 2.

[0038] Table 2. Corrosion resistance test results of Examples 1, 5 and Comparative Examples 4-5

[0039] It can be seen from the data in Table 2 that the data in Example 5 is lower than that in Example 1, indicating that the prepared corrosion-resistant coating can effectively improve the corrosion resistance of the nickel-based alloy. It can be seen from the data in Example 5 and Comparative Example 4 that the addition of 2-(1,3-benzothiazole-2-thio)succinic acid as a corrosion inhibitor effectively improves the corrosion resistance of the coating. It can be seen from the data in Example 5 and Comparative Example 5 that the introduction of lubricant polytetrafluoroethylene enhances the corrosion resistance of the coating.

[0040] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A nickel-based corrosion-resistant alloy, characterized in that: The nickel-based alloy composition is: C≤0.005wt%, 0.04-0.08wt%Si, 0.3-0.8wt%Mn, 14.5-16.5wt%Cr, 15-17wt%Mo, 3.0-4.5wt%W, 4-7wt%Fe, Co≤1.5wt%, 0.1-0.2wt%V, 0.01-0.05wt%Ce, 0.05-0.1wt%Er, 0.05-0.2wt%Hf, 0.003-0.006wt%P, and the balance is Ni and unavoidable impurities.

2. The method for preparing a nickel-based corrosion-resistant alloy according to claim 1, characterized in that: The steps include: Step 1: Preparation of solid block of hafnium boride Boric acid and citric acid are mixed and added to hafnium oxide nanopowder, and then ball-milled and sintered to finally obtain a hafnium boride solid block; Step 2: Preparation of mixed powder Firstly, the raw materials except the hafnium boride solid block are melted and refined, and then the hafnium boride solid block is added for further refining to prepare a vacuum ingot, which is then forged, rolled and heat treated to finally obtain a nickel-based alloy.

3. The method for preparing a nickel-based corrosion-resistant alloy according to claim 2, characterized in that: Step 1 Preparation of hafnium boride solid block specifically includes the following steps: Step 1.1: dissolving 3-3.5 parts by weight of boric acid and 0.5-0.7 parts by weight of citric acid in 8-10 parts by weight of deionized water, stirring at 80-100° C. for 3-5 hours to obtain a mixed solution; Step 1.2: Add 1-2 parts by weight of hafnium oxide nanopowder to the mixed solution, mix and stir to form a slurry, and place the slurry in a planetary ball mill to obtain a prefabricated slurry; Step 1.3: The prefabricated slurry is first dried and then placed in a tubular furnace for sintering. The temperature is increased and then kept warm under vacuum to finally obtain a solid block of hafnium boride.

4. The method for preparing a nickel-based corrosion-resistant alloy according to claim 3, characterized in that: Step 2: Preparation of nickel-based alloy, specifically comprising the following steps: Step 2.1: The nickel-based alloy composition is: C≤0.005wt%, 0.04-0.08wt%Si, 0.3-0.8wt%Mn, 14.5-16.5wt%Cr, 15-17wt%Mo, 3.0-4.5wt%W, 4-7wt%Fe, Co≤1.5wt%, 0.1-0.2wt%V, 0.01-0.05wt%Ce, 0.05-0.1wt%Er, 0.05-0.2wt%Hf, 0.003-0.006wt%P, and the balance is Ni and unavoidable impurities; Step 2.2: according to the above ratio, the raw materials except the solid block of hafnium boride are melted, refined at 1530-1550°C for 20-30min, the solid block of hafnium boride is added, and the heat preservation and stirring treatment is continued for 20-30min, and the casting temperature is 1510-1530°C to obtain a vacuum ingot; Step 2.3: The vacuum ingot is subjected to electroslag remelting, forging, rolling, and heat treatment to finally obtain a nickel-based alloy.

5. The method for preparing a nickel-based corrosion-resistant alloy according to claim 3, characterized in that: The specific parameters of the temperature-keeping after heating under vacuum state in step 1.3 are heating to 650-700°C and keeping for 0.5-1h, then heating to 1100-1150°C and keeping for 2h, and then heating to 1550-1600°C and keeping for 2-3h.

6. The method for preparing a nickel-based corrosion-resistant alloy according to claim 4, characterized in that: The smelting time in step 2.2 is 1 to 2 hours.

7. The method for preparing a nickel-based corrosion-resistant alloy according to claim 2, characterized in that: The method also includes spraying a corrosion-resistant coating on a nickel-based alloy, comprising the following steps: Step I: Preparation of corrosion-resistant coating The corrosion-resistant coating is prepared by using an organic resin binder, a corrosion inhibitor, a lubricant and a mixed solvent; Step II: Preparation of nickel-based corrosion-resistant alloy The prepared corrosion-resistant coating is sprayed evenly on the rough surface of the nickel-based alloy by a spraying process, and the nickel-based corrosion-resistant alloy is obtained after curing.

8. The method for preparing a nickel-based corrosion-resistant alloy according to claim 7, characterized in that: Step I: Preparation of corrosion-resistant coating, specifically comprising the following steps: Step I.I: dissolving 20-30 parts by weight of novolac epoxy resin and 10-20 parts by weight of phenolic resin in 50-80 parts by weight of a mixed solvent, stirring evenly to obtain a solution I, wherein the mixed solvent is ethylene glycol ethyl ether, butanone and toluene in a volume ratio of 5:3:10; Step I.II: grind and disperse 30-50 parts by weight of polytetrafluoroethylene powder through a cone mill, add it to 30-50 parts by weight of a mixed solvent, mix well, add 2-4 parts by weight of 2-(1,3-benzothiazole-2-thio)succinic acid, stir and disperse at 300-500 r / min for 10-20 minutes, and obtain solution II; Step I.III: Mix solution I and solution II and mix them evenly with a high-speed stirrer to obtain a corrosion-resistant coating.

9. The method for preparing a nickel-based corrosion-resistant alloy according to claim 8, characterized in that: Step II: Preparation of nickel-based corrosion-resistant alloy, specifically comprising the following steps: Step II.I: After removing grease, scale, pollutants, etc. from the surface of the nickel-based alloy, mechanical grinding is performed for 20-30 seconds to obtain a nickel-based alloy with a rough surface; Step II.II: The coating is evenly sprayed on the rough surface of the nickel-based alloy by a spraying process, and the coating is solidified after being dried to obtain a nickel-based corrosion-resistant alloy.

10. The method for preparing a nickel-based corrosion-resistant alloy according to claim 9, characterized in that: The curing conditions in step II.II are: curing at 190-195°C for 1.5-2h.

Citation Information

Cited By

  • Rapidly-solidified nickel-based alloy wire and preparation process thereof

    CN121610685A

  • A rapidly solidified nickel-based alloy wire and a process for making the same