Production method of rare earth lanthanum microalloyed 600MPa-grade high-strength steel bar
Through the combination of vanadium nitrogen plus trace niobium microalloyation and rare earth lanthanum elements, combined with post-rolling and cooling technology, the strength and cost of HRB600 steel bars are solved, and the high strength and corrosion resistance are improved, meeting the user's use needs .
Patent Information
- Application Number
- CN202410935619.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing HRB600 steel bars have poor mechanical strength, unstable performance, and high production costs, making it difficult to meet the needs of increasing strength and reducing costs.
Using vanadium nitrogen plus trace niobium microalloy combined with post-rolling controlled cooling production method, and adding rare earth lanthanum elements, chemical composition and process parameters are controlled through converter smelting, LF ladle refining and continuous casting processes to ensure high strength and corrosion resistance of steel bars performance.
The rare earth lanthanum microalloyed high-strength steel bars produced meet the standards of 650MPa yield strength and 780MPa tensile strength, achieving low-cost processes, and improving the corrosion resistance of the steel bars.
Smart Images

Figure BDA0004941235240000031 
Figure BDA0004941235240000041 
Figure BDA0004941235240000042
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a production method of a rare earth lanthanum microalloyed 600MPa grade high-strength steel bar. Background Art
[0002] HRB600 is the grade of threaded steel bar specified in "Steel for Reinforced Concrete" GB 1499.2-2018. Due to the wide range of standard composition and the differences in production equipment and process control of manufacturers, the composition of HRB600 hot-rolled ribbed steel bars produced by various manufacturers is different, and the production processes of various steel mills are also different. The existing HRB600 steel bars have poor mechanical strength and unstable performance. In order to improve the strength of the steel bars and reduce production costs, the present invention adopts vanadium nitrogen and trace niobium microalloying combined with post-rolling controlled cooling to produce HRB600 steel bars, and adds rare earth lanthanum elements to improve the corrosion resistance of the steel bars. Summary of the invention
[0003] The purpose of the present invention is to provide a method for producing a rare earth lanthanum microalloyed 600MPa grade high-strength steel bar.
[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0005] The present invention discloses a method for producing a rare earth lanthanum microalloyed 600MPa grade high-strength steel bar, comprising:
[0006] Converter smelting: The basicity of the final slag of the combined blowing converter is controlled at 2.0, and the end point control target is that the C content is not less than 0.06wt%, and the tapping temperature is ≥1620℃;
[0007] LF ladle refining: argon blowing is carried out throughout the refining process according to the refining procedures, desulfurization, composition fine-tuning and temperature raising operations are carried out according to the composition and temperature of the converter molten steel, and VN16 alloy and rare earth lanthanum alloy are added in the later stage of refining;
[0008] Continuous casting process: superheat is set at 25-35℃, pulling speed is 2.1-2.3m / min; rolling, starting temperature is 1010-1030℃, and final rolling temperature is 850-900℃;
[0009] The chemical composition of the alloy is as follows: C 0.26-0.28%, Si 0.60-0.70%, Mn 1.50-1.60%, V 0.13-0.14%, Nb 0.02-0.03%, the amount of rare earth La added is 30 ppm, and the balance is Fe and unavoidable impurities.
[0010] Further, its chemical composition in mass percentage is: C 0.26%, Si 0.67%, Mn 1.53%, V 0.13%, Nb 0.021%, La 15ppm, P, 0.015%, S 0.012%, and the balance is Fe and inevitable impurities.
[0011] Further, its chemical composition in mass percentage is: C 0.27%, Si 0.68%, Mn 1.54%, V 0.14%, Nb 0.023%, La 16ppm, P, 0.022%, S 0.022%, and the balance is Fe and inevitable impurities.
[0012] Furthermore, in LF furnace refining, auxiliary materials are added to make slag according to the composition and temperature changes of molten steel, and alloys are added for fine-tuning and temperature-raising operations; 300kg of lime, bauxite and vanadium-nitrogen alloy are added, and silicon-calcium wire is fed after refining, with a feed amount of 200-300m3.
[0013] Furthermore, the mechanical properties meet the following requirements: yield strength ≥ 650 MPa, tensile strength ≥ 780 MPa.
[0014] Compared with the prior art, the beneficial technical effects of the present invention are:
[0015] All indicators of the rare earth lanthanum microalloyed high-strength steel bars produced by the present invention meet standard requirements and can meet the needs of users. The steel bars are produced by a medium-high carbon vanadium-nitrogen process and a low-cost process is achieved by controlled cooling after rolling. DETAILED DESCRIPTION
[0016] The present invention will be further described below in conjunction with the embodiments.
[0017] Two heats of steel were produced in industrial trial production, and the specific process parameters were controlled as follows:
[0018] 1. Converter smelting
[0019] During converter smelting, lime, dolomite and iron balls are added according to the component requirements, and ferrosilicon and silicon manganese are added during the steelmaking process.
[0020] The carbon content, phosphorus content (mass percentage) and tapping temperature of the molten steel at the converter end point are shown in Table 1.
[0021] Table 1 Composition and temperature of steel tapping from converter
[0022] Steel tapping temperature, ℃ Carbon content of steel, wt% Phosphorus content of steel, wt% Example 1 1625 0.08 0.021 Example 2 1626 0.07 0.022
[0023] 2. LF furnace refining
[0024] According to the composition and temperature changes of molten steel, auxiliary materials are added to make slag, and alloys are added for fine adjustment and temperature increase. Add 300kg of lime, bauxite, and vanadium nitrogen alloy, and feed the silicon calcium wire after refining, with a feeding amount of 200-300m, and add 30kg of rare earth lanthanum alloy at the same time.
[0025] 3. Continuous casting production
[0026] The process parameters are listed in Table 2; the product components are listed in Table 3.
[0027] Table 2 Continuous casting process parameters
[0028] Superheat(℃) Pulling speed(m / min) Example 1 34 2.1 Example 2 35 2.1
[0029] Table 3 Finished product composition (wt%, balance iron)
[0030]
[0031] 4. Steel rolling production
[0032] The production size is Φ20mm steel bars; the starting rolling temperature is 1010-1030℃, and the final rolling temperature is 850-900℃. After rolling, the controlled cooling water tank starts a water pump at 1350 rpm.
[0033] Table 4 Rolling process parameters
[0034]
[0035] The steel bars prepared in the above three embodiments were tested for mechanical properties, and the test results are listed in Table 5:
[0036] Table 5 Mechanical properties test
[0037]
[0038] As can be seen from Table 5, all indicators of the rare earth lanthanum microalloyed high-strength steel bars produced by the present invention meet the standard requirements and can meet the needs of users. The steel bars are produced by a medium-high carbon vanadium-nitrogen process and a low-cost process is achieved by controlled cooling after rolling.
[0039] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for producing a rare earth lanthanum microalloyed 600MPa grade high-strength steel bar, characterized in that: include: Converter smelting: The basicity of the final slag of the combined blowing converter is controlled at 2.0, and the end point control target is that the C content is not less than 0.06wt%, and the tapping temperature is ≥1620℃; LF ladle refining: argon blowing is carried out in accordance with the refining procedures throughout the process, desulfurization, composition fine-tuning and temperature raising operations are carried out according to the composition and temperature of the converter molten steel, and VN16 alloy and rare earth lanthanum alloy are added in the later stage of refining; Continuous casting process: superheat is set at 25-35℃, pulling speed is 2.1-2.3m / min; rolling, starting temperature is 1010-1030℃, and final rolling temperature is 850-900℃; The chemical composition of the alloy by mass percentage is: C 0.26-0.28%, Si 0.60-0.70%, Mn 1.50-1.60%, V0.13-0.14%, Nb 0.02-0.03%, the addition amount of the rare earth La element is 30ppm, and the balance is Fe and inevitable impurities.
2. The method for producing rare earth lanthanum microalloyed 600 MPa grade high-strength steel bars according to claim 1, characterized in that: Its chemical composition in mass percentage is: C 0.26%, Si 0.67%, Mn 1.53%, V 0.13%, Nb 0.021%, La 15ppm, P, 0.015%, S 0.012%, and the balance is Fe and unavoidable impurities.
3. The method for producing rare earth lanthanum microalloyed 600 MPa grade high-strength steel bars according to claim 1, characterized in that: Its chemical composition in mass percentage is: C 0.27%, Si 0.68%, Mn 1.54%, V 0.14%, Nb 0.023%, La 16ppm, P, 0.022%, S 0.022%, and the balance is Fe and inevitable impurities.
4. The method for producing rare earth lanthanum microalloyed 600 MPa grade high-strength steel bars according to claim 1, characterized in that: In LF furnace refining, auxiliary materials are added to make slag according to the composition and temperature changes of molten steel, and alloys are added for fine-tuning and temperature-raising operations; 300kg of lime, bauxite and vanadium-nitrogen alloy are added, and the silicon-calcium wire is fed after refining, with a feed amount of 200-300m3.
5. The method for producing rare earth lanthanum microalloyed 600 MPa grade high-strength steel bars according to claim 1, characterized in that: Mechanical properties meet the following requirements: yield strength ≥ 650MPa, tensile strength ≥ 780MPa.
Citation Information
Patent Citations
HRB600 high-strength hot-rolling ribbed reinforcing bars with added ferro-silicon nitride and manufacturing method thereof
CN110306116A
635MPa-grade high-strength anti-seismic steel bar and preparation method thereof
CN111945074A
600MPa-grade corrosion-resistant rare earth steel bar and production method thereof
CN113061805A
640MPa-grade high-strength aseismic steel bar and preparation method thereof
CN115198197A
Production method of rare earth microalloyed fine grain HRB400 reinforcing steel bar
CN117568696A