Oxygen and aluminum control method for smelting low-carbon low-silicon steel

By using a two-step method in the converter and LF furnace for smelting low-carbon and low-silicon steel, combined with aluminum-manganese alloy, slag lime and calcium wire, the precise control of oxygen activity and aluminum content in the molten steel is achieved, and the existing technology is solved The precise control problem during the smelting process reduces the smelting cost and improves product quality.

CN118957414APending Publication Date: 2024-11-15GANSU JIU STEEL GRP HONGXING IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411195910.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to accurately control the oxygen activity and aluminum content in the molten steel during the smelting of low-carbon and low-silicon steel, resulting in the prone to subcutaneous bubbles, cracks, high inclusions and continuous casting machine flocculation, especially in the absence of RH furnaces. Among enterprises with equipment and silicon deoxygenation capabilities, smelting costs will also increase.

Method used

The two-step method of converter depth deoxygenation and LF furnace segment control is adopted. By adding aluminum-ferromanganese alloy to the converter and using slag lime and steel slag modification agent in the LF furnace, combined with calcium wire feeding, the oxygen activity in the molten steel is accurately controlled. The degree and aluminum content avoid repeated adjustments of the argon blowing station and the LF refining furnace.

Benefits of technology

The precise control of oxygen activity and aluminum content in molten steel is achieved, which reduces smelting costs, avoids subcutaneous bubbles, cracks and continuous casting machine flocculation, and ensures the purity and low silicon content of molten steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides an oxygen control and aluminum control method for smelting low-carbon low-silicon steel, which comprises the following steps: (1) converter deep deoxidation: adding an aluminum-manganese-iron alloy into a steel ladle during converter tapping, mixing with molten steel, and carrying out deep precipitation deoxidation on the molten steel; (2) controlling dissolved oxygen of molten steel in an LF furnace in a segmented manner, adding the molten steel in a steel ladle into the LF furnace, adding slag lime into the LF furnace, heating for the first time, and then adding a steel slag modifier for heating for the second time; and (3) calcium wires are fed into the molten steel, so that the calcium-aluminum ratio in the molten steel is 0.08-0.11. According to the method, oxygen and aluminum are controlled step by step through the converter and the LF refining furnace, silicon deoxidation is not used, meanwhile, repeated adjustment of the oxygen activity of the molten steel through aluminum feeding wires of an argon blowing station and the LF refining furnace is avoided, the oxygen activity and the aluminum content in the molten steel are accurately controlled through two-step deoxidation operation, and the silicon content of the molten steel is controlled to be 0.02% or below.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy and relates to a method for controlling oxygen and aluminum in smelting low-carbon and low-silicon steel. Background Art

[0002] In low-carbon, low-silicon steel, C is usually controlled to be ≤ 0.08% and Si is ≤ 0.03%. Therefore, silicon deoxidation cannot be used and aluminum deoxidation is used. Its typical steel grades are the welding rod steel series, H08A, H08C, H08E and other steel grades. Due to their special composition properties, small square billet casting is extremely difficult. If the oxygen activity in the molten steel is too high, it is easy to cause surface defects such as subcutaneous bubbles and cracks, affecting the steel quality; if the oxygen activity is low, the aluminum content in the molten steel is high, and the inclusions are high, it is easy to cause flocculence in the continuous casting machine.

[0003] In the prior art, for the special properties of low-carbon and low-silicon steel, most of the methods for controlling the oxygen activity of molten steel in one step are adopted. For example, the invention with publication number 117265209 discloses a method for producing H08A steel by steelmaking. The method uses an RH furnace to further treat the molten steel to further reduce the [O] content of the molten steel, improve product quality, and reduce alloy costs. However, the method is only applicable to large and medium-sized converters for producing H08A. It cannot be applied to enterprises without RH furnace equipment, and vacuum treatment causes an increase in smelting costs. The invention with publication number 111235351 A discloses a method for controlling the oxygen content in molten steel during smelting. According to the oxygen content in the converter molten steel and the target alloy element content requirements, a certain amount of ferrosilicon alloy and metallic manganese are added to the ladle after the furnace, and a certain amount of lime slag-making agent is added to the ladle after the steel is discharged. The LF arrival temperature is above 1560°C. After the molten steel enters the LF refining furnace, the oxygen content can be controlled between 30 and 50 ppm. However, the method uses silicon deoxidation and cannot be applied to steel grades with Si≤0.03% or lower. The invention with publication number 116770016 A discloses a method for accurately controlling the oxygen activity of low-carbon, low-aluminum, sulfur-containing steel in an LF refining furnace. This method stably controls the oxygen activity content in the molten steel at the end of smelting in the LF furnace between 40ppm and 60ppm through the mass transfer balance at the slag-steel interface, and can achieve long-term stable pouring of continuous casting. However, this method uses silicon carbide deoxidation in the LF furnace, and can only control Si≤0.05% in the molten steel, and cannot meet the requirements of steel grades with Si≤0.03% or lower. In addition, the papers "H08A Steel Two-Step Silicon Control and Oxygen Control Production Practice" and "LD-LF-CC Process Smelting H08A Process Development" both describe the production of H08A steel using the converter-LF refining-small billet continuous casting process. Production practice has shown that controlling the oxygen activity of molten steel in the converter or argon blowing station and LF refining furnace can solve surface defects such as subcutaneous bubbles and cracks and the problem of flocculence in the continuous casting machine. However, in actual production, it is still necessary to feed aluminum wire in the argon blowing station or LF refining furnace, and repeatedly adjust the oxygen activity of the molten steel, and it is impossible to accurately control the oxygen activity and aluminum content in the molten steel. Summary of the invention

[0004] The purpose of the present invention is to provide a method for controlling oxygen and aluminum in smelting low-carbon and low-silicon steel in response to the problems existing in the prior art.

[0005] To this end, the present invention adopts the following technical solutions: A method for controlling oxygen and aluminum in smelting low-carbon and low-silicon steel comprises the following steps: (1) Deep deoxidation in the converter: when tapping steel from the converter, aluminum-manganese-iron alloy is added to the ladle and mixed with the molten steel to perform deep precipitation deoxidation on the molten steel. The tapping temperature of the converter is 1640-1680°C, and the oxygen activity of the molten steel is 0.040-0.075% when tapping steel. (2) The LF furnace controls the dissolved oxygen of molten steel in stages. The molten steel in the ladle is added to the LF furnace and slag lime is added to the LF furnace and the temperature is raised to 1590-1610°C for the first time. The amount of slag lime added is 6-12 kg / t. After the heating is completed, the oxygen is determined, and then the slag modification agent is added to heat the temperature to 1610-1630°C for the second time. After the second heating, the oxygen activity of the molten steel is 0.003-0.005%; (3) Calcium wire is fed into the molten steel so that the calcium-aluminum ratio in the molten steel is 0.08-0.11.

[0006] Furthermore, the amount of aluminum-manganese-iron alloy added in step (1) is 铝锰铁 Calculated according to the following formula: M 铝锰铁 =(2×27×(ω[O] 初始 -ω[O] 目标 ) / 3×16×η1×η2)×M 钢水量 ×1000 In the formula, ω[O] 初始 is the oxygen content in the molten steel at the end of the converter, ω[O] 目标 is the target controlled oxygen content in the converter molten steel, η1 is the aluminum content in the Al-Mn-Fe alloy, and η2 is the deoxidation efficiency of the aluminum element in the Al-Mn-Fe alloy.

[0007] Furthermore, in the step (1), high-draw supplementary blowing or one-time carbon drawing is used to control the oxygen activity of the molten steel.

[0008] Furthermore, the mass percentages of various substances in the aluminum-manganese-iron alloy in step (1) are Al≥17%, Mn≥28%, and the rest are Fe and unavoidable impurities.

[0009] Furthermore, in the step (2), argon is blown into the bottom of the molten steel for 2 minutes before oxygen determination.

[0010] Furthermore, in step (2), if the oxygen activity of the molten steel detected by oxygen determination is not greater than 0.003%, the amount of steel slag added is 0.3 kg / t; if the oxygen activity of the molten steel detected by oxygen determination is between 0.003% and 0.004%, the amount of steel slag added is 0.4 kg / t; if the oxygen activity of the molten steel detected by oxygen determination is between 0.004% and 0.005%, the amount of steel slag added is 0.5 kg / t.

[0011] Furthermore, the mass percentages of various substances in the steel slag modifier in the step (2) are as follows: Al ≥ 40%, SiO2 ≤ 3.0%, Al2O3: 15% to 30%, CaO: 10% to 35%, P ≤ 0.05%, S ≤ 0.1%, H2O ≤ 1.0%, and the rest are unavoidable impurities. The particle size of the steel slag modifier is 5 to 50 mm.

[0012] The beneficial effects of the present invention are as follows: oxygen and aluminum are controlled in steps by using a converter and an LF refining furnace, silicon deoxidation is not used, and repeated adjustment of the oxygen activity of the molten steel by an argon blowing station and an aluminum feeding line of the LF refining furnace is avoided. The oxygen activity and aluminum content in the molten steel are accurately controlled through a two-step deoxidation operation, and the silicon content of the molten steel is controlled to be below 0.02%, thereby solving the problem of subcutaneous bubbles, cracks, high inclusions, low purity of the molten steel, and flocculence of the continuous casting machine in producing low-carbon and low-silicon steel by using a converter-LF refining-small square billet continuous casting process. DETAILED DESCRIPTION

[0013] The present invention is described in detail below in conjunction with embodiments: Example 1 This embodiment is applied to a process of a 50-ton converter-LF furnace-150×150 small square billet continuous casting machine in a certain factory. The smelting steel grade is H08A, the molten steel volume is 50 tons, and the target composition of the finished product is shown in Table 1: Table 1 (1) Deep deoxidation in the converter. When the converter is tapping, an aluminum-manganese-iron alloy is added to the ladle and mixed with the molten steel to perform deep precipitation deoxidation on the molten steel. When the converter is tapping, the C content is 0.04%, the tapping temperature is 1647°C, and the high-draw supplementary blowing method is used to control the oxygen activity of the molten steel to 0.043%. Specifically, the mass percentages of various substances in the aluminum-manganese-iron alloy are Al: 20.2%, Mn: 32.4%, and the rest are Fe and unavoidable impurities. The amount of aluminum-manganese-iron alloy added is calculated according to the following formula: M 铝锰铁 =(2×27×(ω[O] 初始 -ω[O] 目标 ) / 3×16×η1×η2)×M 钢水量 ×1000 In the formula, ω[O] 初始is the oxygen content in the molten steel at the end of the converter, which is 0.043% in this embodiment, ω[O] 目标 is the target controlled oxygen content in the converter steel water, which is 0.0015% in this embodiment, η1 is the aluminum content in the aluminum-manganese-iron alloy, which is 20.2% in this embodiment, η2 is the deoxidation efficiency of the aluminum element in the aluminum-manganese-iron alloy, which is 60% in this embodiment, and M 钢水量 It is 50t. Through calculation, it can be obtained that 192.6Kg of aluminum-manganese-iron alloy is put into the ladle, and 150kg of ladle synthetic slag can be produced after deoxidation of the aluminum-manganese-iron alloy.

[0014] (2) The LF furnace controls the dissolved oxygen of molten steel in sections. The molten steel in the ladle is added to the LF furnace. The temperature of the molten steel entering the station is 1568℃. The oxygen activity of the molten steel is 0.0018% when the oxygen is measured. The T[Al] in the molten steel is 0.0023% when the sample entering the station is analyzed. Silicon deoxidation is not used, and the repeated adjustment of the oxygen activity of the molten steel by the argon blowing station and the aluminum feeding line of the LF refining furnace is avoided. The purity of the molten steel is ensured by deep deoxidation of the steel tapping from the converter. Then slag lime is added to the LF furnace. The addition of slag lime The amount is 6-12Kg / t, that is, 6-12Kg of slag lime is added to each ton of molten steel. In this embodiment, 300kg, i.e. 6Kg / t, is added. At the same time, 100kg of fluorite is added to the molten steel, so that the LF furnace slag forms primary slag as soon as possible while ensuring that the final slag basicity is greater than 3.5, reducing the activity of SiO2 in the slag, and then heating to 1593°C for the first time, controlling the oxygen activity of the molten steel [O] ≤ 0.005%. After the heating is completed, the molten steel is subjected to oxygen determination detection. In the embodiment, the oxygen activity of the molten steel [O] = 0.0027%. Since the oxygen activity of the molten steel detected by oxygen determination is not more than 0.003%, the amount of steel slag modifier added is 0.3kg / t. Therefore, 15kg of steel slag modifier is added to the molten steel for the second heating to 1621°C. The mass percentages of various substances in the steel slag modifier in this embodiment are Al: 46%, SiO2: 1.7%, Al2O3: 30%, CaO: 27%, P: 0.03%, S: 0.05%, H2O: 0.8%, and the rest are inevitable impurities. The particle size of the slag modifier is 5-50 mm. The slag modifier is used for diffusion deoxidation to ensure a reducing atmosphere. After the second heating, the oxygen activity of the molten steel is 0.003-0.005%. In this embodiment, the oxygen activity of the molten steel is 0.0043%, and the temperature measured by the thermocouple is 1622°C. The TAl in the molten steel is 0.0039%. The composition of the molten steel after the LF refining furnace in this embodiment is shown in Table 2: Table 2 (3) Calcium wire is fed into the molten steel to make the calcium-aluminum ratio in the molten steel be 0.08-0.11. In this embodiment, the [Al] content is 0.0035%. 45 m of calcium wire is fed, and the calcium-aluminum ratio is controlled to be 0.10. After feeding the calcium wire, the soft blowing time is 10 min. The temperature is measured with a thermocouple at 1609 ° C. This avoids repeated feeding of aluminum wire into the LF furnace. The aluminum content in the molten steel is low, and Al2O3 inclusions are controlled from the source.

[0015] The molten steel is hoisted into small square billets of 150×150mm for casting, with a casting speed of 2.4m / min and a mid-term temperature of the tundish of 1541℃. Due to the two-step method for precise oxygen and aluminum control, there is no flocculence in the casting, and there are no defects such as pores and cracks on the surface of the billet.

[0016] Example 2 A two-step method for accurately controlling oxygen and aluminum in smelting low-carbon and low-silicon steel in this embodiment is applied to a 50-ton converter-LF furnace-150×150 small square billet continuous casting machine process in a certain factory, smelting steel grade H08A, with a molten steel volume of 50 tons. The target composition of the finished product is shown in Table 3 below: Table 3 (1) Deep deoxidation in the converter. When the converter is tapping, an aluminum-manganese-iron alloy is added to the ladle and mixed with the molten steel to perform deep precipitation deoxidation on the molten steel. When the converter is tapping, the C content is 0.05%, the tapping temperature is 1662°C, and the high-draw supplementary blowing method is used to control the oxygen activity of the molten steel to 0.055%. Specifically, the mass percentages of various substances in the aluminum-manganese-iron alloy are Al: 21.5%, Mn: 29.3%, and the rest are Fe and unavoidable impurities. The amount of aluminum-manganese-iron alloy added is calculated according to the following formula: M 铝锰铁 =(2×27×(ω[O] 初始 -ω[O] 目标 ) / 3×16×η1×η2)×M 钢水量 ×1000 In the formula, ω[O] 初始 is the oxygen content in the molten steel at the end of the converter, which is 0.043% in this embodiment, ω[O] 目标 is the target controlled oxygen content in the converter steel water, which is 0.0015% in this embodiment, η1 is the aluminum content in the aluminum-manganese-iron alloy, which is 21.5% in this embodiment, η2 is the deoxidation efficiency of the aluminum element in the aluminum-manganese-iron alloy, which is 60% in this embodiment, and M 钢水量 It is 50t. Through calculation, it can be obtained that 233.3Kg of aluminum-manganese-iron alloy is put into the ladle, and 150kg of ladle synthetic slag can be produced after deoxidation of the aluminum-manganese-iron alloy.

[0017] (2) The LF furnace controls the dissolved oxygen of molten steel in sections. The molten steel in the ladle is added to the LF furnace. The temperature of the molten steel entering the station is 1583℃. The oxygen activity of the molten steel is 0.0031% when the oxygen is measured. The T[Al] in the molten steel is 0.0030% when the sample entering the station is analyzed. Silicon deoxidation is not used, and the repeated adjustment of the oxygen activity of the molten steel by the argon blowing station and the aluminum feeding line of the LF refining furnace is avoided. The purity of the molten steel is ensured by deep deoxidation of the steel tapping from the converter. Then slag lime is added to the LF furnace. The amount of slag lime added is 6-12Kg / t, that is, 6-12Kg of slag lime is added to each ton of molten steel. In this embodiment, 400kg, i.e. 8Kg / t, is added. At the same time, 150Kg of fluorite is added to the molten steel, so that the LF furnace slag forms primary slag as soon as possible while ensuring that the final slag basicity is greater than 3.5, reducing the activity of SiO2 in the slag, and then heating to 1602℃ for the first time, controlling the oxygen activity of the molten steel [O] ≤ 0.005%. After the heating is completed, the molten steel is subjected to oxygen determination detection. In this embodiment, In this example, the oxygen activity of molten steel [O] = 0.0032%. Since the oxygen activity of molten steel detected by oxygen determination is 0.003-0.004%, the amount of steel slag modifier added is 0.4 kg / t. Therefore, 20 kg of steel slag modifier is added to the molten steel for the second heating to 1614 ° C. The mass percentages of various substances in the steel slag modifier in this embodiment are: Al: 50%, SiO2: 1.2%, Al2O3: 25%, CaO: 25%, P: 0.03%, S :0.05%,H2O:0.8%,the rest are inevitable impurities. The particle size of the slag modifier is 5~50mm. The slag modifier is used for diffusion deoxidation to ensure the reducing atmosphere. After the second heating, the oxygen activity of the molten steel is 0.003~0.005%. In this embodiment, the oxygen activity of the molten steel is 0.0038%, and the temperature measured by the thermocouple is 1622℃. The TAl in the molten steel is 0.0031%. The composition of the molten steel after the LF refining furnace treatment in this embodiment is shown in Table 4: Table 4 (3) Calcium wire is fed into the molten steel to make the calcium-aluminum ratio in the molten steel be 0.08-0.11. In this embodiment, the [Al] content is 0.0036%. 50 m of calcium wire is fed and the calcium-aluminum ratio is controlled to be 0.10. After feeding the calcium wire, the soft blowing time is 10 min. The temperature is measured at 1612°C with a thermocouple, thereby avoiding repeated feeding of aluminum wire into the LF furnace. The aluminum content in the molten steel is low, and Al2O3 inclusions are controlled at the source.

[0018] The molten steel is hoisted into small square billets of 150×150mm for casting, with a casting speed of 2.4m / min and a mid-term temperature of the tundish of 1545℃. Due to the two-step method for precise oxygen and aluminum control, there is no flocculence in the casting, and there are no defects such as pores and cracks on the surface of the billet.

[0019] Example 3 A two-step method for accurately controlling oxygen and aluminum in smelting low-carbon and low-silicon steel in this embodiment is applied to a 50-ton converter-LF furnace-150×150 small square billet continuous casting machine process in a certain factory, smelting steel grade H08A, with a molten steel volume of 50 tons. The target composition of the finished product is shown in Table 5 below: Table 5 (1) Deep deoxidation in the converter. When the converter is tapping, an aluminum-manganese-iron alloy is added to the ladle and mixed with the molten steel to perform deep precipitation deoxidation on the molten steel. When the converter is tapping, the C content is 0.04%, the tapping temperature is 1662°C, and the high-draw supplementary blowing method is used to control the oxygen activity of the molten steel to 0.060%. Specifically, the mass percentages of various substances in the aluminum-manganese-iron alloy are Al: 120.2%, Mn: 30.2%, and the rest are Fe and unavoidable impurities. The amount of aluminum-manganese-iron alloy added is calculated according to the following formula: M 铝锰铁 =(2×27×(ω[O] 初始 -ω[O] 目标 ) / 3×16×η1×η2)×M 钢水量 ×1000 In the formula, ω[O] 初始 is the oxygen content in the molten steel at the end of the converter, which is 0.060% in this embodiment, ω[O] 目标 is the target controlled oxygen content in the converter steel water, which is 0.0015% in this embodiment, η1 is the aluminum content in the aluminum-manganese-iron alloy, which is 19.5% in this embodiment, η2 is the deoxidation efficiency of the aluminum element in the aluminum-manganese-iron alloy, which is 60% in this embodiment, and M 钢水量 It is 50t. Through calculation, it can be obtained that 281.3Kg of aluminum-manganese-iron alloy is put into the ladle, and 150kg of ladle synthetic slag can be produced after deoxidation of the aluminum-manganese-iron alloy.

[0020] (2) The LF furnace controls the dissolved oxygen of molten steel in sections. The molten steel in the ladle is added to the LF furnace. The temperature of the molten steel entering the station is 1554℃. The oxygen activity of the molten steel is 0.0012% when the oxygen is measured. The T[Al] in the molten steel is 0.0040% when the sample entering the station is analyzed. Silicon deoxidation is not used, and the repeated adjustment of the oxygen activity of the molten steel by the argon blowing station and the aluminum feeding wire of the LF refining furnace is avoided. The steel is deeply deoxidized by the converter to ensure the purity of the molten steel. Then, slag lime is added to the LF furnace. The amount of slag lime added is 6-1 2Kg / t, that is, 6-12Kg of slag lime is added to each ton of molten steel. In this embodiment, 500kg, i.e. 10Kg / t, is added. At the same time, 200Kg of fluorite is added to the molten steel, so that the LF furnace slag forms primary slag as soon as possible while ensuring that the final slag basicity is greater than 3.5, reducing the activity of SiO2 in the slag, and then heating to 1609℃ for the first time, controlling the oxygen activity of the molten steel [O] ≤ 0.005%. After the heating is completed, the molten steel is subjected to oxygen determination. In this embodiment, the oxygen activity of the molten steel is [O]=0.0043%. Since the oxygen activity of molten steel detected by oxygen determination is 0.004%-0.005%, the amount of steel slag modifier added is 0.5kg / t. Therefore, 25kg of steel slag modifier is added to the molten steel for the second heating to 1619°C. The mass percentages of various substances in the steel slag modifier in this embodiment are Al: 50%, SiO2: 1.5%, Al2O3: 27%, CaO: 19%, P: 0.03%, S: 0.05%, H2O: 0.8%, the rest are inevitable impurities, the particle size of the steel slag modifier is 5-50mm, the steel slag modifier is used for diffusion deoxidation to ensure a reducing atmosphere, after the second heating is completed, the oxygen activity of the molten steel is 0.003-0.005%, in this embodiment, the oxygen activity of the molten steel is 0.0032%, the TAl in the molten steel is 0.0049%, the composition after the LF refining furnace treatment in this embodiment is shown in Table 2 below, the temperature measured by a thermocouple is 1620°C, and the composition of the molten steel after the LF refining furnace treatment is shown in Table 6: Table 6 (3) Calcium wire is fed into the molten steel to make the calcium-aluminum ratio in the molten steel be 0.08-0.11. In this embodiment, the [Al] content is 0.0049%. 55 m of calcium wire is fed and the calcium-aluminum ratio is controlled to be 0.10. After feeding the calcium wire, the soft blowing time is 10 min. The temperature is measured at 1605°C using a thermocouple. This avoids repeated feeding of aluminum wire into the LF furnace. The aluminum content in the molten steel is low, and Al2O3 inclusions are controlled at the source.

[0021] The molten steel is hoisted into small square billets of 150×150mm for casting, with a casting speed of 2.4m / min and a mid-term temperature of the tundish of 1541℃. Due to the two-step method for precise oxygen and aluminum control, there is no flocculence in the casting, and there are no defects such as pores and cracks on the surface of the billet.

Claims

1. A method for controlling oxygen and aluminum in smelting low-carbon and low-silicon steel. It is characterized in that The following steps are involved: (1) Deep deoxidation in the converter: when tapping steel from the converter, aluminum-manganese-iron alloy is added to the ladle and mixed with the molten steel to perform deep precipitation deoxidation on the molten steel. The tapping temperature of the converter is 1640-1680°C, and the oxygen activity of the molten steel is 0.040-0.075% when tapping steel. (2) The LF furnace controls the dissolved oxygen of molten steel in stages. The molten steel in the ladle is added to the LF furnace and slag lime is added to the LF furnace and the temperature is raised to 1590-1610°C for the first time. The amount of slag lime added is 6-12 kg / t. After the heating is completed, the oxygen is determined, and then the slag modification agent is added to heat the temperature to 1610-1630°C for the second time. After the second heating, the oxygen activity of the molten steel is 0.003-0.005%; (3) Calcium wire is fed into the molten steel so that the calcium-aluminum ratio in the molten steel is 0.08-0.

11.

2. A method for controlling oxygen and aluminum in smelting low-carbon and low-silicon steel according to claim 1, It is characterized in that The amount of aluminum-manganese-iron alloy added in step (1) is M 铝锰铁 Calculated according to the following formula: M 铝锰铁 =(2×27×(ω[O] 初始 -ω[O] 目标 ) / 3×16×η 1 ×h 2 )×M 钢水量 ×1000 In the formula, ω[O] 初始 is the oxygen content in the molten steel at the end of the converter, ω[O] 目标 To control the oxygen content in the converter steel water, η 1 is the aluminum content in the aluminum-manganese-iron alloy, η 2 It is the deoxidation efficiency of aluminum element in aluminum-manganese-iron alloy.

3. The method for controlling oxygen and aluminum in smelting low-carbon and low-silicon steel according to claim 1, It is characterized in that In the step (1), high-draw supplementary blowing or one-time carbon drawing is used to control the oxygen activity of the molten steel.

4. The method for controlling oxygen and aluminum in smelting low-carbon and low-silicon steel according to claim 1, It is characterized in that The mass percentages of various substances in the aluminum-manganese-iron alloy in step (1) are Al≥17%, Mn≥28%, and the rest are Fe and unavoidable impurities.

5. The method for controlling oxygen and aluminum in smelting low-carbon and low-silicon steel according to claim 1, It is characterized in that In the step (2), argon is blown into the bottom of the molten steel for 2 minutes before oxygen is determined.

6. The method for controlling oxygen and aluminum in smelting low-carbon and low-silicon steel according to claim 1, It is characterized in that In the step (2), if the oxygen activity of the molten steel detected by oxygen determination is not greater than 0.003%, the amount of steel slag added is 0.3 kg / t; if the oxygen activity of the molten steel detected by oxygen determination is between 0.003% and 0.004%, the amount of steel slag added is 0.4 kg / t; if the oxygen activity of the molten steel detected by oxygen determination is between 0.004% and 0.005%, the amount of steel slag added is 0.5 kg / t.

7. The method for controlling oxygen and aluminum in smelting low-carbon and low-silicon steel according to claim 1, It is characterized in that The mass percentages of various substances in the steel slag modifier in step (2) are: Al≥40%, SiO 2 ≤3.0%,Al 2 O 3 : 15%~30%, CaO: 10%~35%, P≤0.05%, S≤0.1%, H 2 O≤1.0%, the rest are inevitable impurities, and the particle size of the slag modifier is 5~50mm.