Negative electrode current collector Fe-Ni alloy foil and preparation method thereof
By optimizing the electrodeposition method and electrolyte composition, Fe-Ni alloy foil with excellent mechanical properties of Fe-Ni alloy foil was prepared, which solved the poor mechanical properties of Fe-Ni alloy foil and the adjustable Fe and Ni content of Fe and Ni in the prior art. The poor performance problem increases the cycle life and energy density of the battery.
Patent Information
- Application Number
- CN202410945912.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-15
AI Technical Summary
In the prior art, the Fe-Ni alloy foil has poor mechanical properties, low tensile strength and poor controllability of Fe and Ni content, resulting in cracks and active substances easily disengagement during battery preparation, affecting the battery cycle life.
The Fe-Ni alloy foil was prepared by electrodeposition method. By optimizing the composition of the electrolyte and the electrodeposition parameters, the Fe and Ni content were controlled between 35 and 65%, the thickness was 3-10μm, the tensile strength was greater than 1.5GPa, and the elongation was controlled. More than 5%, and through screening of additives and current density, an alloy foil with excellent mechanical properties is formed.
The mechanical properties of Fe-Ni alloy foil are improved, and the tensile strength and elongation are significantly improved, which solves the problems of cracks and active substances in the current collector in the battery, extends the cycle life of the battery, and increases the energy density of the battery.
Smart Images

Figure CN118957430A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of Fe-Ni alloy foil, in particular to a negative electrode current collector Fe-Ni alloy foil and a preparation method thereof. Background Art
[0002] Fe-Ni alloy is widely used because of its excellent magnetic properties and low expansion coefficient. It can be used as iron core material, magnetic shielding material, magnetostrictive material, magnetic storage material, lead frame material, battery skeleton material, etc. It has become an important part of new materials and high technology, and Fe-Ni alloy foil has better mechanical properties than pure iron foil and pure nickel foil. Fe-Ni alloy foil is obtained by replacing part of the precious metal nickel with low-cost iron. Its corrosion resistance is equivalent to that of bright nickel, and its toughness is better than that of bright nickel, so it can save nickel resources and effectively reduce costs.
[0003] There are few studies on Fe-Ni alloy foil prepared by electrodeposition in the prior art, especially Fe-Ni alloy foil with high mechanical properties. China Invention Patent Publication No. CN108559915A discloses "A Fe-Ni alloy and its preparation method", and the tensile strength of the prepared alloy foil is between 810 and 880 MPa; China Invention Patent Publication No. CN108166024A discloses "A process for preparing Fe-Ni alloy foil by electrodeposition", and the current density range is small and narrow, only 3.6-4.0 A / dm 2 , which is significantly different from the production current, and the tensile strength of the prepared alloy foil is less than 800MPa; Patent CN107805761B discloses "an iron-nickel alloy foil and its manufacturing method", and the Fe-Ni content in the prepared Fe-Ni alloy foil can be controlled in a narrow range, and the tensile strength is between 1.0 and 1.5GPa.
[0004] It can be seen that the Fe-Ni alloy prepared by the existing electrodeposition method has low tensile strength and poor controllability of the Fe and Ni contents in the plating solution; in terms of low tensile strength, during the battery preparation process, the current collector (Fe-Ni alloy foil) coated with active materials will undergo flattening, winding and other processes. If the tensile strength and elongation are low, cracks, separation from the active materials, and reduced battery cycle life are likely to occur; in terms of poor controllability, due to the different electrodeposition potentials of Fe and Ni, Fe is deposited preferentially, and the preparation of Fe-Ni belongs to co-deposition. If it is not regulated, it will result in less Ni deposition or no Ni deposition. Summary of the invention
[0005] In view of the deficiencies of the above-mentioned prior art, the object of the present invention is to provide a negative electrode current collector Fe-Ni alloy foil and a preparation method thereof. The present invention aims to solve the technical problems in the prior art that the Fe-Ni alloy foil has poor mechanical properties and poor production controllability of the Fe and Ni contents, and to provide a Fe-Ni alloy foil with excellent mechanical properties and controllable Fe and Ni contents.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] A negative electrode current collector Fe-Ni alloy foil, in which the mass percentage of iron is 35-65%, the mass percentage of nickel is 35-65%, and the sum of the mass percentages of the two is ≥99% and less than or equal to 100%, and the remainder is impurities.
[0008] Preferably, the thickness of the Fe-Ni alloy foil is 3-10 μm, and the thickness is measured with a micrometer. Compared with the prior art, the Fe-Ni alloy foil of the present invention is thinner. The Fe-Ni alloy is used for the negative electrode current collector. When the thickness is thinner, the proportion of the Fe-Ni alloy in the battery is smaller. Under the condition that the volume of the battery cell remains unchanged, the amount of active material can be increased, and the slurry coating thickness is thickened, which directly promotes the improvement of the energy density of the battery cell. Therefore, the thinner the Fe-Ni alloy foil, the greater the effect on improving the energy density of the battery. The lowest thickness disclosed in the currently known patents is 5 μm, and when the thickness of the Fe-Ni alloy foil of the present invention is 3 μm, the mechanical properties are higher than those of the known patents proposed in the background technology.
[0009] Preferably, the tensile strength of the Fe-Ni alloy foil is greater than 1.5 GPa, and the elongation is greater than 5%.
[0010] The present invention also provides a method for preparing the above-mentioned negative electrode current collector Fe-Ni alloy foil, which comprises the following steps:
[0011] By using the electrodeposition method, the cathode roller and the anode plate are placed in a reaction tank containing an electrolyte, and the Fe-Ni alloy foil is electrodeposited on the cathode roller. The electrolyte consists of the following components:
[0012] Main salts: FeSO4·7H2O 55~120g / L and NiSO4·6H2O 105~315g / L; further, FeSO4·7H2O 60~110g / L, NiSO4·6H2O 110~300g / L;
[0013] Complexing agent sodium citrate 3-10g / L; further, sodium citrate 3-8g / L; complexing agent can form a stable and uniform complex with metal ions, change the properties and behavior of metal ions, and prevent Fe 3+ Formation of Fe(OH)3 precipitate;
[0014] Buffer: boric acid 6-40 g / L; further, boric acid 6-35 g / L; the buffer is used to adjust the pH balance of the plating solution;
[0015] Antioxidant ascorbic acid 3-15 g / L; further, ascorbic acid 3-10 g / L; Antioxidant is used to prevent Fe 2+ Oxidized to Fe 3+ ;
[0016] The additives include two or more of saccharin sodium 3-15 g / L, sodium dodecyl sulfate 0.1-2 g / L, polydisulfide dipropane sulfonate sodium 0.5-2 ppm, collagen 0.5-5 ppm, hydroxyethyl cellulose 0.5-5 ppm, polyethylene glycol 20000 0.5-5 ppm, HCl 3-24 ml / L, and NaCl 5-30 g / L. The additives are used to change the cathode polarization, thereby changing the mechanical properties, micromorphology and apparent state of the alloy foil.
[0017] Furthermore, two or more of saccharin sodium 3-12 g / L, sodium dodecyl sulfate 0.1-1.5 g / L, collagen 0.5-3 ppm, hydroxyethyl cellulose 0.5-3 ppm, polyethylene glycol 20000 0.5-2 ppm, HCl 3-20 ml / L, and NaCl 5-25 g / L.
[0018] Preferably, the electrolyte is prepared according to the following steps:
[0019] After the buffer is stirred and dissolved in heated pure water, the main salt, chelating agent and antioxidant are added in turn and stirred and dissolved, and finally the additives are added and the temperature is adjusted to 30-60°C. The temperature has little effect on the iron and nickel content, but too high a temperature affects the foil formation, and the index is slightly low. If the temperature is too low, the reaction is more violent, the solution resistance increases, and the power loss is large; the pH is adjusted to 1.9-2.9 to obtain an electrolyte; further, the solution preparation temperature is 40-55°C, and the solution pH is 2.0-2.7; too high or too low a temperature and pH affect the foil appearance, mechanical properties, micromorphology and Fe and Ni content of the coating.
[0020] Preferably, the pH is adjusted using a 5% by volume sulfuric acid solution or a 5% by mass NaOH solution.
[0021] Preferably, the steps of the electrodeposition method are:
[0022] Put the cathode roller that has been polished with sandpaper and preheated into the electrolytic cell. The sandpaper used for polishing the cathode roller is 1000-1500#. Adjust the electroplating stirring speed and cathode current density, and control the electroplating time. Pass direct current to electro-deposit Fe-Ni alloy foil. After the electro-deposition is completed, take out the cathode roller and wash it twice with water, blow dry it, and peel it off from the cathode to obtain Fe-Ni alloy foil.
[0023] Preferably, the electrodeposition parameters are: stirring speed 30-80rpm, too high stirring speed will cause violent reaction and affect foil formation; too low speed will affect the iron-nickel content of the coating, reduce the Fe content, reduce the elongation, and the elongation is less than 5%; cathode current density 10-35A / dm 2 , electroplating time is 70 to 150s; time affects the thickness of the Fe-Ni alloy foil. When the current is determined, the shorter the time, the thinner the foil, and the longer the time, the thicker the foil.
[0024] Furthermore, the stirring speed is 30-70 rpm, and the cathode current density is 10-30 A / dm 2 , electroplating time 70 ~ 140s.
[0025] Preferably, the cathode roller for electrodeposition is a pure titanium roller, and the anode plate is a titanium-iridium-plated anode plate, and both the cathode roller and the anode plate for electrodeposition are obtained after screening.
[0026] Preferably, the preheating temperature of the cathode roller is 30-60° C., and the electrolyte temperature will not be lowered when the cathode roller is placed in the electrolyte after preheating, and no pinholes are generated in the formed foil after the cathode roller is preheated.
[0027] Furthermore, the cathode roller is preheated in pure water to a temperature of 40 to 55°C.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. An ultra-thin Fe-Ni alloy foil with good mechanical properties, smooth surface morphology and a thickness of 3-10 μm is prepared by the method of the present invention. The tensile strength of the Fe-Ni alloy foil is greater than 1.5 GPa and the elongation is greater than 5%. During the preparation of the battery, the current collector (Fe-Ni alloy foil) coated with active materials needs to go through processes such as flattening and winding. If the tensile strength and elongation are low, cracks are likely to occur and the foil is separated from the active materials, thereby reducing the battery cycle life. The Fe-Ni alloy foil provided by the present invention has excellent mechanical properties and overcomes the technical defects of the existing current collectors.
[0030] 2. The Fe-Ni alloy foil prepared by the present invention has an iron content of 35-65%, a nickel content of 35-65%, and an impurity content of less than 1%. The Fe and Ni contents in the alloy foil are highly controllable and can be controlled according to the requirements of the battery. Different contents exhibit different mechanical properties and can be reasonably controlled according to requirements.
[0031] 3. The present invention provides a method for preparing Fe-Ni alloy foil used as a negative electrode current collector for a battery. The Fe-Ni alloy foil prepared by this method has strong corrosion resistance and high safety, and can be used as a negative electrode current collector for a battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The tensile strength and elongation of the Fe-Ni alloy foil of Examples 1-3 and Comparative Example 1 of the present invention are shown;
[0033] Figure 2 This is a scanning electron microscope image of the Fe-Ni alloy foil of Example 1 of the present invention;
[0034] Figure 3 is a scanning electron microscope image of the Fe-Ni alloy foil of Example 2 of the present invention;
[0035] Figure 4 This is a scanning electron microscope image of the Fe-Ni alloy foil of Example 3 of the present invention;
[0036] Figure 5 This is a scanning electron microscope image of the Fe-Ni alloy foil of Comparative Example 1 of the present invention;
[0037] Figure 6 This is a physical picture of the Fe-Ni alloy foil of Comparative Example 2 of the present invention;
[0038] Figure 7 This is a scanning electron microscope image of the Fe-Ni alloy foil of Comparative Example 3 of the present invention;
[0039] Figure 8 This is a physical picture of the Fe-Ni alloy foil of Comparative Example 4 of the present invention;
[0040] Fig. 9 In the figure, (a) is a physical picture of the Fe-Ni alloy foil of comparative example 5 of the present invention, and (b) is a scanning electron microscope picture of the Fe-Ni alloy foil of comparative example 5 of the present invention;
[0041] Fig.10 This is a scanning electron microscope image of the Fe-Ni alloy foil of Comparative Example 6 of the present invention;
[0042] Fig.11 This is a scanning electron microscope image of the Fe-Ni alloy foil of Comparative Example 7 of the present invention;
[0043] Fig.12In the figure, (a) is an electron microscope image of Fe-Ni alloy foil, (b) is an EDS spectrum analysis image, and (b) is the spectrum image of the selected position in (a);
[0044] Fig.13 It is a comparison chart of corrosion resistance, wherein the left picture is copper foil and the right picture is Fe-Ni alloy foil of Example 1 of the present invention. DETAILED DESCRIPTION
[0045] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention. The experimental methods described in the embodiments of the present invention are conventional methods unless otherwise specified.
[0046] The present invention can prepare an alloy foil with controllable Fe and Ni contents by regulating the electrolyte components in the plating solution, namely, the main salt concentration, additives, complexing agents, antioxidants and buffers, and considering the Fe 2+ Easily oxidized to Fe 3+ The present invention can make Fe 2+ Stable in solution;
[0047] The Fe-Ni alloy foil of the present invention has excellent mechanical properties. As far as the mechanical properties are concerned, the present invention creatively adopts additives, screens the amount of additives, and screens the current density. Under the combined effect of additives and current density, an Fe-Ni alloy foil with excellent mechanical properties is obtained.
[0048] The experimental conditions provided by the present invention are obtained through screening, and the study found that only when the mass percentage of iron is 35-65% and the mass percentage of nickel is 35-65%, can a Fe-Ni alloy foil with a tensile strength greater than 1.5 GPa and an elongation greater than 5% be obtained, that is, a Fe-Ni alloy foil with excellent mechanical properties be obtained; a comparative study using comparative examples shows that conditions not within the scope of this application cannot obtain a Fe-Ni alloy foil with excellent mechanical properties. The following examples and comparative examples are used to study the technical solution of this application, as shown below:
[0049] Example 1
[0050] A method for preparing a negative electrode current collector Fe-Ni alloy foil, wherein the mass percentage of the alloy foil is: 49.76% iron and 49.66% nickel, comprising the following steps:
[0051] (1) Solution preparation:
[0052] Stir and dissolve the weighed boric acid in pure water at 40°C, then add NiSO4·6H2O in sequence, stir and dissolve, add sodium citrate, stir and dissolve, add ascorbic acid, stir and dissolve, add FeSO4·7H2O, stir and dissolve, then add NaCl and sodium saccharin, stir and dissolve, and finally adjust the pH to 2.0 with a 5% by volume sulfuric acid solution to obtain an electrolyte;
[0053] The specific components of the electrolyte are: FeSO4·7H2O 85g / L, NiSO4·6H2O 275g / L, sodium citrate 3g / L, boric acid 8g / L, ascorbic acid 5g / L, sodium saccharin 3g / L, NaCl 10g / L;
[0054] (2) Electrodeposition process:
[0055] The electrolyte of step (1) was poured into the electrolytic cell, with the titanium cathode roller as the cathode and the titanium iridium-plated anode plate as the anode. The cathode roller polished with 1200# sandpaper and preheated at 40°C was placed in the electrolytic cell as the cathode. The electroplating stirring speed was adjusted to 40 rpm and the cathode current density was adjusted to 25 A / dm 2 The electroplating time is 80s, and direct current is passed to electro-deposit Fe-Ni alloy foil. After the electro-deposition is completed, the cathode roller is taken out, and it is washed twice, blown dry, and peeled to obtain Fe-Ni alloy foil. Its microstructure is as follows Figure 2 As shown, the thickness is 5 μm.
[0056] Example 2
[0057] A method for preparing a negative electrode current collector Fe-Ni alloy foil, wherein the mass percentage of the alloy foil is: 63.78% iron and 36.01% nickel, comprising the following steps:
[0058] (1) Solution preparation:
[0059] The weighed boric acid was stirred and dissolved in pure water at 50°C, and then NiSO4·6H2O was added in sequence to stir and dissolve, sodium citrate was added to stir and dissolve, ascorbic acid was added to stir and dissolve, FeSO4·7H2O was added to stir and dissolve, and then HCl, sodium polydisulfide propane sulfonate and sodium saccharin were added to stir and dissolve, and finally the pH was adjusted to 2.7 with 5% by volume sodium hydroxide to obtain an electrolyte;
[0060] The specific components of the electrolyte are: FeSO4·7H2O 100g / L, NiSO4·6H2O 305g / L, sodium citrate 5g / L, boric acid 25g / L, ascorbic acid 3g / L, sodium saccharin 8g / L, sodium polydisulfide dipropane sulfonate 0.5ppm, HCl 10mL / L;
[0061] (2) Electrodeposition process:
[0062] The electrolyte of step (1) was poured into the electrolytic cell, with the titanium cathode roller as the cathode and the titanium iridium-plated anode plate as the anode. The cathode roller polished with 1200# sandpaper and preheated at 50°C was placed in the electrolytic cell as the cathode. The electroplating stirring speed was adjusted to 60 rpm and the cathode current density was adjusted to 30 A / dm 2 The electroplating time is 70s, and direct current is passed to electro-deposit Fe-Ni alloy foil. After the electro-deposition is completed, the cathode roller is taken out, and it is washed twice, blown dry, and peeled to obtain Fe-Ni alloy foil. Its microstructure is as follows Figure 3 As shown, the thickness is 5 μm.
[0063] Example 3
[0064] A method for preparing a negative electrode current collector Fe-Ni alloy foil, wherein the mass percentage of the alloy foil is: 35.45% iron and 64.24% nickel, comprising the following steps:
[0065] (1) Solution preparation:
[0066] Stir and dissolve the weighed boric acid in pure water at 50°C, then add NiSO4·6H2O in sequence, stir and dissolve, add sodium citrate, stir and dissolve, add ascorbic acid, stir and dissolve, add FeSO4·7H2O, stir and dissolve, then add NaCl, sodium dodecyl sulfate, collagen and sodium saccharin, stir and dissolve, and finally adjust the pH to 2.4 with 5% by volume dilute sulfuric acid to obtain an electrolyte;
[0067] The specific components of the electrolyte are: FeSO4·7H2O 65g / L, NiSO4·6H2O 285g / L, sodium citrate 3g / L, boric acid 18g / L, ascorbic acid 5g / L, saccharin sodium 10g / L, sodium dodecyl sulfate 1g / L, collagen 2ppm, NaCl 20g / L;
[0068] (2) Electrodeposition process:
[0069] The electrolyte of step (1) was poured into the electrolytic cell, with the titanium cathode roller as the cathode and the titanium iridium-plated anode plate as the anode. The cathode roller polished with 1200# sandpaper and preheated at 50°C was placed in the electrolytic cell as the cathode. The electroplating stirring speed was adjusted to 30 rpm and the cathode current density to 30 A / dm 2 The electroplating time is 70s, and direct current is passed to electro-deposit Fe-Ni alloy foil. After the electro-deposition is completed, the cathode roller is taken out, and it is washed twice, blown dry, and peeled to obtain Fe-Ni alloy foil. Its microstructure is as follows Figure 4 As shown, the thickness is 5 μm.
[0070] Example 4
[0071] A method for preparing a negative electrode current collector Fe-Ni alloy foil, wherein the mass percentage of the alloy foil is: 38.21% iron and 61.14% nickel, comprising the following steps:
[0072] (1) Solution preparation:
[0073] Stir and dissolve the weighed boric acid in pure water at 50°C, then sequentially add NiSO4·6H2O and stir and dissolve, add sodium citrate and stir and dissolve, add ascorbic acid and stir and dissolve, add FeSO4·7H2O and stir and dissolve, then add hydroxyethyl cellulose and polyethylene glycol 2000 and stir and dissolve, and finally adjust the pH to 2.9 with 5% by volume dilute sulfuric acid to obtain an electrolyte;
[0074] The specific components of the electrolyte are: FeSO4·7H2O 55g / L, NiSO4·6H2O 105g / L, sodium citrate 4g / L, boric acid 6g / L, ascorbic acid 4g / L, hydroxyethyl cellulose 0.5g / L, polyethylene glycol 20005ppm;
[0075] (2) Electrodeposition process:
[0076] The electrolyte of step (1) was poured into the electrolytic cell, with the titanium cathode roller as the cathode and the titanium iridium-plated anode plate as the anode. The cathode roller, which had been polished with 1200# sandpaper and preheated at 50°C, was placed in the electrolytic cell as the cathode. The electroplating stirring speed was adjusted to 30 rpm and the cathode current density to 35 A / dm 2 , the electroplating time is 100s, direct current is passed to electro-deposit Fe-Ni alloy foil. After the electro-deposition is completed, the cathode roller is taken out, and it is washed twice, blown dry, and peeled to obtain Fe-Ni alloy foil.
[0077] Example 5
[0078] A method for preparing a negative electrode current collector Fe-Ni alloy foil, wherein the mass percentage of the alloy foil is: 54.60% iron and 44.81% nickel, comprising the following steps:
[0079] (1) Solution preparation:
[0080] Stir and dissolve the weighed boric acid in pure water at 50°C, then add NiSO4·6H2O in sequence, stir and dissolve, add sodium citrate, stir and dissolve, add ascorbic acid, stir and dissolve, add FeSO4·7H2O, stir and dissolve, then add sodium dodecyl sulfate and sodium saccharin, stir and dissolve, and finally adjust the pH to 1.9 with 5% by volume dilute sulfuric acid to obtain an electrolyte;
[0081] The specific components of the electrolyte are: FeSO4·7H2O 120g / L, NiSO4·6H2O 315g / L, sodium citrate 10g / L, boric acid 40g / L, ascorbic acid 15g / L, sodium saccharin 15g / L, sodium dodecyl sulfate 2g / L;
[0082] (2) Electrodeposition process:
[0083] The electrolyte of step (1) was poured into the electrolytic cell, with the titanium cathode roller as the cathode and the titanium iridium-plated anode plate as the anode. The cathode roller polished with 1500# sandpaper and preheated at 50°C was placed in the electrolytic cell as the cathode. The electroplating stirring speed was adjusted to 80 rpm and the cathode current density was adjusted to 10 A / dm 2 , the electroplating time is 150s, direct current is passed to electro-deposit Fe-Ni alloy foil. After the electro-deposition is completed, the cathode roller is taken out, and it is washed twice, blown dry, and peeled to obtain Fe-Ni alloy foil.
[0084] Comparative Example 1
[0085] A method for preparing a negative electrode current collector Fe-Ni alloy foil, the preparation steps of this comparative example are the same as those of Example 1, except that FeSO4·7H2O is replaced from 85 g / L to 40 g / L, and NiSO4·6H2O is replaced from 275 g / L to 350 g / L, that is, the amount of FeSO4·7H2O in the main salt is replaced to be lower than the lower limit, and the amount of NiSO4·6H2O is replaced to be higher than the upper limit, and the mass percentage of the obtained Fe-Ni alloy foil is: 18.78% iron, 80.42% nickel, comprising the following steps:
[0086] (1) Solution preparation:
[0087] Stir and dissolve the weighed boric acid in pure water at 50°C, then add NiSO4·6H2O in sequence, stir and dissolve, add sodium citrate, stir and dissolve, add ascorbic acid, stir and dissolve, add FeSO4·7H2O, stir and dissolve, then add sodium saccharin, stir and dissolve, and finally adjust the pH to 2.0 with 5% by volume dilute sulfuric acid to obtain an electrolyte;
[0088] The specific components of the electrolyte are: FeSO4·7H2O 40g / L, NiSO4·6H2O 350g / L, sodium citrate 3g / L, boric acid 8g / L, ascorbic acid 5g / L, sodium saccharin 3g / L, NaCl 10g / L;
[0089] (2) Electrodeposition process:
[0090] The electrolyte of step (1) was poured into the electrolytic cell, with the titanium cathode roller as the cathode and the titanium iridium-plated anode plate as the anode. The cathode roller polished with 1200# sandpaper and preheated at 50°C was placed in the electrolytic cell as the cathode. The electroplating stirring speed was adjusted to 40 rpm and the cathode current density was adjusted to 25 A / dm 2 , the electroplating time is 80s, direct current is passed to electro-deposit Fe-Ni alloy foil, after the electro-deposition is completed, the cathode roller is taken out, and it is washed twice, blown dry, and peeled off to obtain Fe-Ni alloy foil with a thickness of 5μm;
[0091] Since the amount of FeSO4·7H2O in this comparative example is lower than the scope of this application, and the amount of NiSO4·6H2O is higher than the scope of this application, the Ni content of the Fe-Ni alloy foil is greater than 65%, and the iron content is less than 35%. Its microscopic morphology is as follows Figure 5 As shown, Figure 5 The electron microscope showed that there were many nodular particles in the Fe-Ni alloy foil and the foil surface was uneven. The tensile strength of the obtained Fe-Ni alloy foil was 0.88 GPa and the elongation was 4.3%. At this time, the mechanical properties did not meet the requirements, with a tensile strength of <1.5 GPa and an elongation of <5%.
[0092] Comparative Example 2
[0093] A method for preparing a negative electrode current collector Fe-Ni alloy foil, the preparation steps of this comparative example are the same as those of Example 1, except that FeSO4·7H2O is replaced from 85 g / L to 150 g / L, and NiSO4·6H2O is replaced from 275 g / L to 95 g / L, that is, the amount of FeSO4·7H2O in the main salt is replaced to be higher than the upper limit, and the amount of NiSO4·6H2O is replaced to be lower than the lower limit, comprising the following steps:
[0094] (1) Solution preparation:
[0095] Stir and dissolve the weighed boric acid in pure water at 50°C, then add NiSO4·6H2O in sequence, stir and dissolve, add sodium citrate, stir and dissolve, add ascorbic acid, stir and dissolve, add FeSO4·7H2O, stir and dissolve, then add sodium saccharin, stir and dissolve, and finally adjust the pH to 2.0 with 5% by volume dilute sulfuric acid to obtain an electrolyte;
[0096] The specific components of the electrolyte are: FeSO4·7H2O 150g / L, NiSO4·6H2O 95g / L, sodium citrate 3g / L, boric acid 8g / L, ascorbic acid 5g / L, sodium saccharin 3g / L, NaCl 10g / L;
[0097] (2) Electrodeposition process:
[0098] The electrolyte of step (1) was poured into the electrolytic cell, with the titanium cathode roller as the cathode and the titanium iridium-plated anode plate as the anode. The cathode roller polished with 1200# sandpaper and preheated at 50°C was placed in the electrolytic cell as the cathode. The electroplating stirring speed was adjusted to 40 rpm and the cathode current density was adjusted to 25 A / dm 2 , the electroplating time is 80s, direct current is passed to electro-deposit Fe-Ni alloy foil, after the electro-deposition is completed, the cathode roller is taken out, and washed with water twice and blown dry;
[0099] Since the amount of FeSO4·7H2O in this comparative example is higher than the scope of this application, and the amount of NiSO4·6H2O is lower than the scope of this application, the Fe content of the Fe-Ni alloy foil is greater than 65%, and the Ni content is less than 35%. At this time, the foil cannot be formed and cannot be peeled off, and the content determination is meaningless. Therefore, the content determination is not carried out, so there is no mechanical property data. The results are as follows Figure 6 shown.
[0100] Comparative Example 3
[0101] A method for preparing a negative electrode current collector Fe-Ni alloy foil, the preparation steps are the same as those in Example 1, the only difference is that the current value is changed below the lower limit, that is, the current is changed from 25A / dm 2 Replaced with 5A / dm 2 , including the following steps:
[0102] (1) Solution preparation:
[0103] Stir and dissolve the weighed boric acid in pure water at 40°C, then add NiSO4·6H2O in sequence, stir and dissolve, add sodium citrate, stir and dissolve, add ascorbic acid, stir and dissolve, add FeSO4·7H2O, stir and dissolve, then add NaCl and sodium saccharin, stir and dissolve, and finally adjust the pH to 2.0 with a 5% by volume sulfuric acid solution to obtain an electrolyte;
[0104] The specific components of the electrolyte are: FeSO4·7H2O 85g / L, NiSO4·6H2O 275g / L, sodium citrate 3g / L, boric acid 8g / L, ascorbic acid 5g / L, sodium saccharin 3g / L, NaCl 10g / L;
[0105] (2) Electrodeposition process:
[0106] The electrolyte of step (1) was poured into the electrolytic cell, with the titanium cathode roller as the cathode and the titanium iridium-plated anode plate as the anode. The cathode roller polished with 1200# sandpaper and preheated at 40°C was placed in the electrolytic cell as the cathode. The electroplating stirring speed was adjusted to 40 rpm and the cathode current density was adjusted to 5 A / dm 2, the electroplating time is 80s, direct current is passed to electro-deposit Fe-Ni alloy foil, after the electro-deposition is completed, the cathode roller is taken out, and it is washed twice, blown dry, and peeled off to obtain Fe-Ni alloy foil with a thickness of 5μm;
[0107] The results are as follows Figure 7 As shown, Figure 7 The results show that the Fe-Ni alloy foil is well-formed, has obvious color difference from the electron microscope, and has relatively coarse nodular particles. The mechanical properties are poor, with a tensile strength of <1.5GPa and an elongation of <5%.
[0108] Comparative Example 4
[0109] A method for preparing a negative electrode current collector Fe-Ni alloy foil, the preparation steps are the same as those in Example 1, the only difference is that the current is changed to be higher than the upper limit, that is, the current is changed from 25A / dm 2 Replaced with 45A / dm 2 , including the following steps:
[0110] (1) Solution preparation:
[0111] Stir and dissolve the weighed boric acid in pure water at 40°C, then add NiSO4·6H2O in sequence, stir and dissolve, add sodium citrate, stir and dissolve, add ascorbic acid, stir and dissolve, add FeSO4·7H2O, stir and dissolve, then add NaCl and sodium saccharin, stir and dissolve, and finally adjust the pH to 2.0 with a 5% by volume sulfuric acid solution to obtain an electrolyte;
[0112] The specific components of the electrolyte are: FeSO4·7H2O 85g / L, NiSO4·6H2O 275g / L, sodium citrate 3g / L, boric acid 8g / L, ascorbic acid 5g / L, sodium saccharin 3g / L, NaCl 10g / L;
[0113] (2) Electrodeposition process:
[0114] The electrolyte of step (1) was poured into the electrolytic cell, with the titanium cathode roller as the cathode and the titanium iridium-plated anode plate as the anode. The cathode roller polished with 1200# sandpaper and preheated at 40°C was placed in the electrolytic cell as the cathode. The electroplating stirring speed was adjusted to 40 rpm and the cathode current density was adjusted to 45 A / dm 2 , the electroplating time is 80s, direct current is passed to electro-deposit Fe-Ni alloy foil, after the electro-deposition is completed, the cathode roller is taken out, and it is washed twice, blown dry, and peeled off to obtain Fe-Ni alloy foil with a thickness of 5μm;
[0115] The results are as follows Figure 8 As shown, Figure 8 The results show that when the current exceeds the upper limit, the foil cannot be formed and the structure becomes a debris.
[0116] Comparative Example 5
[0117] A method for preparing a negative electrode current collector Fe-Ni alloy foil, which has the same preparation steps as those in Example 1, except that the amount of the additives is regulated so that the amount of saccharin sodium is 1 g / L and the amount of NaCl is 4 g / L, that is, the amount of the additives is less than the lower limit, comprising the following steps:
[0118] (1) Solution preparation:
[0119] Stir and dissolve the weighed boric acid in pure water at 50°C, then add NiSO4·6H2O in sequence, stir and dissolve, add sodium citrate, stir and dissolve, add ascorbic acid, stir and dissolve, add FeSO4·7H2O, stir and dissolve, then add sodium saccharin, stir and dissolve, and finally adjust the pH to 2.0 with 5% by volume dilute sulfuric acid to obtain an electrolyte;
[0120] The specific components of the electrolyte are: FeSO4·7H2O 85g / L, NiSO4·6H2O 275g / L, sodium citrate 3g / L, boric acid 8g / L, ascorbic acid 5g / L, sodium saccharin 1g / L, NaCl 4g / L;
[0121] (2) Electrodeposition process:
[0122] The electrolyte of step (1) was poured into the electrolytic cell, with the titanium cathode roller as the cathode and the titanium iridium-plated anode plate as the anode. The cathode roller polished with 1200# sandpaper and preheated at 50°C was placed in the electrolytic cell as the cathode. The electroplating stirring speed was adjusted to 40 rpm and the cathode current density was adjusted to 25 A / dm 2 , the electroplating time is 80s, direct current is passed to electro-deposit Fe-Ni alloy foil, after the electro-deposition is completed, the cathode roller is taken out, and it is washed twice, blown dry, and peeled off to obtain Fe-Ni alloy foil with a thickness of 5μm;
[0123] like Fig. 9 As shown in the figure, when the amount of additives is small, the foil-forming property is poor. The selected foil-forming area is subjected to electron microscopy, and the results show that there are many coarse nodular particles on the surface, which is uneven. At this time, the Fe content is 20.86% and the Ni content is 78.88%. It can be seen that even if the amounts of FeSO4·7H2O and NiSO4·6H2O are within the scope of this application, the Fe and Ni contents in the Fe-Ni alloy foil cannot reach the required range due to the reduction in the amount of additives.
[0124] Comparative Example 6
[0125] A method for preparing a negative electrode current collector Fe-Ni alloy foil, changing the pH to 1.5, that is, lowering the pH value below the lower limit, comprises the following steps:
[0126] (1) Solution preparation:
[0127] Stir and dissolve the weighed boric acid in pure water at 50°C, then add NiSO4·6H2O in sequence, stir and dissolve, add sodium citrate, stir and dissolve, add ascorbic acid, stir and dissolve, add FeSO4·7H2O, stir and dissolve, then add sodium saccharin, stir and dissolve, and finally adjust the pH to 1.5 with 5% by volume dilute sulfuric acid to obtain an electrolyte;
[0128] The specific components of the electrolyte are: FeSO4·7H2O 110g / L, NiSO4·6H2O 300g / L, sodium citrate 3g / L, boric acid 20g / L, ascorbic acid 5g / L, sodium saccharin 8g / L, NaCl 10g / L;
[0129] (2) Electrodeposition process:
[0130] The electrolyte of step (1) was poured into the electrolytic cell, with the titanium cathode roller as the cathode and the titanium iridium-plated anode plate as the anode. The cathode roller polished with 1200# sandpaper and preheated at 50°C was placed in the electrolytic cell as the cathode. The electroplating stirring speed was adjusted to 30 rpm and the cathode current density to 30 A / dm 2 , the electroplating time is 70s, direct current is passed to electro-deposit Fe-Ni alloy foil, after the electro-deposition is completed, the cathode roller is taken out, and it is washed twice, blown dry, and peeled off to obtain Fe-Ni alloy foil with a thickness of 5μm;
[0131] The Fe-Ni alloy foil obtained has an Fe content greater than 65%, a Ni content less than 35%, a tensile strength <1.5 GPa, an elongation <5%, and a thickness of 5 μm. Fig.10 The electron microscope shows that there are many nodular particles and the foil surface is uneven. In addition, if the additive in the solution is saccharin sodium, it will precipitate and deposit on the anode plate, thereby reducing the current efficiency.
[0132] Comparative Example 7
[0133] A method for preparing a negative electrode current collector Fe-Ni alloy foil, which has the same preparation steps as those of Comparative Example 6, except that the pH value is changed to 3.0, that is, the pH value is higher than the upper limit, comprises the following steps:
[0134] (1) Solution preparation:
[0135] Stir and dissolve the weighed boric acid in pure water at 50°C, then add NiSO4·6H2O in sequence, stir and dissolve, add sodium citrate, stir and dissolve, add ascorbic acid, stir and dissolve, add FeSO4·7H2O, stir and dissolve, then add sodium saccharin, stir and dissolve, and finally adjust the pH to 3 with 5% by volume dilute sulfuric acid to obtain an electrolyte;
[0136] The specific components of the electrolyte are: FeSO4·7H2O 110g / L, NiSO4·6H2O 300g / L, sodium citrate 3g / L, boric acid 20g / L, ascorbic acid 5g / L, sodium saccharin 8g / L, NaCl 10g / L;
[0137] (2) Electrodeposition process:
[0138] The electrolyte of step (1) was poured into the electrolytic cell, with the titanium cathode roller as the cathode and the titanium iridium-plated anode plate as the anode. The cathode roller polished with 1200# sandpaper and preheated at 50°C was placed in the electrolytic cell as the cathode. The electroplating stirring speed was adjusted to 30 rpm and the cathode current density to 30 A / dm 2 , the electroplating time is 70s, direct current is passed to electro-deposit Fe-Ni alloy foil, after the electro-deposition is completed, the cathode roller is taken out, and it is washed twice, blown dry, and peeled off to obtain Fe-Ni alloy foil with a thickness of 5μm;
[0139] like Fig.11 As shown in the electron microscope image, there are many nodular particles and the foil surface is uneven. At this time, the mechanical properties do not meet the requirements, the tensile strength is <1.5GPa, and the elongation is <5%.
[0140] The present invention adopts an electrodeposition method to prepare Fe-Ni alloy foil, uses a sulfate system as an electrolyte, uses a titanium cathode roller as a cathode, and uses a titanium iridium-plated anode plate as an anode, and prepares the Fe-Ni alloy foil in an electrolytic cell under the action of direct current; the tensile strength and elongation of the prepared Fe-Ni alloy foil are measured by a Shimadzu universal tensile testing machine, and the surface morphology and element content of the Fe-Ni alloy foil are measured by a Hitachi scanning electron microscope and a Bruker X-ray spectrometer.
[0141] Comparison of mechanical properties of Examples 1-3 and Comparative Example 1 Figure 1 As shown, through Figure 1 It can be seen that the tensile strength of the Fe-Ni alloy foil obtained in Examples 1-3 is not much different, and the tensile strength is all greater than 1.5 GPa, and the elongation is all greater than 5%, which is better than Comparative Example 1. It can be seen that the amount of main salt in the electrolyte has a great influence on the mass percentage in the Fe-Ni alloy foil, which in turn affects the mechanical properties of the Fe-Ni alloy foil.
[0142] Figure 2-4 The results show that the Fe-Ni alloy foil of the embodiment has a relatively flat and smooth microstructure, and does not have the coarse crystal particles of the control example.
[0143] The Fe-Ni alloy foil prepared by the present invention has an iron mass percentage of 35-65%, a nickel mass percentage of 30-65%, and an impurity content of less than 1%. The obtained Fe-Ni alloy foil is subjected to the following steps: Fig.12EDS spectrum analysis, the data in Table 1 are obtained:
[0144] Table 1 Relative element content of Fe-Ni alloy foil
[0145] Element Type Wire Intensity (c / s) Atomic percentage (%) Mass percentage unit Error rate - Al Ka 8.74 0.999 .473 wt.% .104 Fe Ka 745.80 45.845 44.860 wt.% .437 Ni Ka 558.88 53.156 54.667 wt.% .620 100.000 100.000 wt.% total
[0146] The present invention also conducted a comparative study on corrosion resistance experiments. The Fe-Ni alloy foil prepared in Example 1 of the present invention was compared with the copper foil used for the battery current collector. The corrosion tests were carried out in acidic solutions. The pH of the acidic solution was 2, Cl - =120g / L, Cl is regulated by NaCl - concentration, pH is regulated by sulfuric acid; e.g. Fig.13 As shown, the results show that the Fe-Ni alloy foil is more stable and basically insoluble, and after immersion for 24 hours, the appearance of the Fe-Ni alloy foil is basically unchanged.
[0147] Those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A negative electrode current collector Fe-Ni alloy foil, characterized in that: In the Fe-Ni alloy foil, the mass percentage of iron is 35-65%, the mass percentage of nickel is 35-65%, and the sum of the mass percentages of the two is ≥99% and less than or equal to 100%.
2. The negative electrode current collector Fe-Ni alloy foil according to claim 1, characterized in that: The Fe-Ni alloy foil has a thickness of 3-10 μm.
3. The negative electrode current collector Fe-Ni alloy foil according to claim 1, characterized in that: The tensile strength of the Fe-Ni alloy foil is greater than 1.5 GPa, and the elongation is greater than 5%.
4. A method for preparing the negative electrode current collector Fe-Ni alloy foil according to claim 1, characterized in that: The steps include: By using the electrodeposition method, the cathode roller and the anode plate are placed in a reaction tank containing an electrolyte, and the Fe-Ni alloy foil is electrodeposited on the cathode roller. The electrolyte consists of the following components: Main salts: FeSO4·7H2O 55~120g / L and NiSO4·6H2O 105~315g / L; Complexing agent sodium citrate 3-10g / L; Buffer boric acid 6-40 g / L; Antioxidant ascorbic acid 3-15 g / L; The additives include two or more of saccharin sodium 3-15 g / L, sodium dodecyl sulfate 0.1-2 g / L, polydisulfide dipropane sulfonate sodium 0.5-2 ppm, collagen 0.5-5 ppm, hydroxyethyl cellulose 0.5-5 ppm, polyethylene glycol 20000 0.5-5 ppm, HCl 3-24 ml / L, and NaCl 5-30 g / L.
5. The method for preparing the negative electrode current collector Fe-Ni alloy foil according to claim 4, characterized in that: The steps of electrodeposition are: The cathode roller polished with sandpaper and preheated is placed in an electrolytic cell, and direct current is passed to electrodeposit Fe-Ni alloy foil. After the electrodeposition is completed, the Fe-Ni alloy foil is peeled off from the cathode to obtain the Fe-Ni alloy foil.
6. The method for preparing the negative electrode current collector Fe-Ni alloy foil according to claim 5, characterized in that: Electrodeposition parameters: stirring speed 30-80 rpm, cathode current density 10-35 A / dm 2 , electroplating time 70 ~ 150s.
7. The method for preparing the negative electrode current collector Fe-Ni alloy foil according to claim 5, characterized in that: The cathode roller preheating temperature is 30-60°C.
8. The method for preparing the negative electrode current collector Fe-Ni alloy foil according to claim 4, characterized in that: The cathode roller of the electrodeposition is a pure titanium roller, and the anode plate is a titanium-iridium-plated anode plate.
9. The method for preparing the negative electrode current collector Fe-Ni alloy foil according to claim 4, characterized in that: The electrolyte is prepared as follows: After the buffer is stirred and dissolved in heated pure water, the main salt, the complexing agent and the antioxidant are added in sequence and stirred and dissolved, and finally the additive is added, and the temperature is adjusted to 30-60°C and the pH to 1.9-2.9 to obtain the electrolyte.
10. The method for preparing the negative electrode current collector Fe-Ni alloy foil according to claim 9, characterized in that: The pH value is adjusted by using a 5% by volume sulfuric acid solution or a 5% by mass NaOH solution.
Citation Information
Patent Citations
Preparation methods of iron-nickel or iron-nickel-chromium alloy foils and the electrolytes used
CN102268703A
Preparation method of iron-nickel-cobalt-molybdenum alloy foil by electrodeposition
CN103243356A
Fe-Ni alloy foil and method for manufacturing the same
CN107805761A
Aluminum-copper-titanium alloy foil for positive current collector and manufacturing method of aluminum-copper-titanium alloy foil
CN114277284A
Process for preparing invor alloy foil
CN1793433A
Cited By
Iron-nickel alloy foil with copper-plated surface and preparation method thereof
CN119980392A
Cathode roller with honeycomb surface structure and method for manufacturing alloy foil by using cathode roller
CN120082936A
Low-crimp iron-nickel alloy foil suitable for all-solid-state battery and preparation method thereof
CN120221672A
Low-curl iron-nickel alloy foil suitable for all-solid-state batteries and preparation method thereof
CN120221672B
Electrolyte for preparing nickel-iron alloy foil and application
CN120758936A