Method for improving elastic property of titanium alloy foil
By optimizing the alloy composition and multi-stage heat treatment process of titanium alloy, the problem of insufficient elastic properties of titanium alloy foil is solved, high elastic strain and high strength material performance is achieved, and the demanding requirements of high-end electronic products are met.
Patent Information
- Application Number
- CN202411064847.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
The elastic properties of existing titanium alloy foils are poor, making it difficult to meet the demand for high-elastic materials for high-end electronic products, especially in devices such as folding screen mobile phones and tablets.
By optimizing the alloy composition of titanium alloy, multi-stage heat treatment and rolling processes are adopted, including preliminary heat treatment, isothermal aging treatment, multi-stage aging treatment, stress elimination treatment, strain induction treatment and stabilization treatment, finely adjusting the microstructure and phase of the alloy Stability, improve the elastic properties of the foil.
It significantly improves the elastic strain of titanium alloy foil to reach more than 1%, meeting the flexible deformation needs of high-end electronic products, and improving the high strength and fatigue resistance of the material.
Smart Images

Figure CN118957465A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal material processing, and in particular to a method for improving the elastic performance of a titanium alloy foil. Background Art
[0002] With the rapid development of consumer electronics, the performance requirements for titanium alloy foils are also increasing. Although the existing titanium alloy foils perform well in terms of strength, there is still room for improvement in terms of elasticity. In addition, the existing conventional titanium alloy plates or bars generally have good elasticity, but after being prepared into foils, the elasticity is poor. The elastic strain of conventional titanium alloy foils is generally less than 0.8%, which is difficult to meet the requirements of flexible deformation. In order to meet the demand for high-elastic titanium alloy foils for 3C electronic products such as folding screen mobile phones and tablets, a new processing heat treatment process is urgently needed to significantly improve the elastic properties of titanium alloy foils.
[0003] Currently, no technical solution is disclosed in the public technology on how to improve the elastic properties of titanium alloy foil. Summary of the invention
[0004] The purpose of the present invention is to provide a method for improving the elastic properties of titanium alloy foil, which can significantly improve the elastic properties of titanium alloy foil through innovative processing and heat treatment technology to meet the stringent requirements of high-end electronic products on materials.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for improving the elastic properties of titanium alloy foil is carried out in the following steps:
[0007] 1. Alloy composition optimization: adjust the content of alloy elements so that the characteristic parameter (η) of the alloy satisfies: 4.14≤η≤4.20; wherein the characteristic parameter (η) of the alloy is calculated according to a specific method;
[0008] The specific method comprises the following steps:
[0009] a. Calculate the atomic percentage (at%) of each element in the titanium alloy, including but not limited to: titanium (Ti), vanadium (V), aluminum (Al), molybdenum (Mo), zirconium (Zr), tin (Sn), niobium (Nb), iron (Fe), manganese (Mn), tantalum (Ta) and chromium (Cr);
[0010] b. Calculate the electron concentration of each element based on the atomic percentage and the number of valence electrons of each element by multiplying the atomic percentage of the element by the number of valence electrons of the element; where the number of valence electrons of each element is as follows:
[0011] Titanium (Ti): 4
[0012] Vanadium(V):5
[0013] Aluminum (Al): 3
[0014] Molybdenum (Mo):6
[0015] Zirconium (Zr): 4
[0016] Tin(Sn):4
[0017] Niobium (Nb): 5
[0018] Iron (Fe): 8
[0019] Manganese (Mn): 7
[0020] Tantalum(Ta):5
[0021] Chromium (Cr): 6
[0022] c. Add the electron concentrations of all elements to obtain the characteristic parameter (η);
[0023] 2. Preliminary heat treatment:
[0024] The alloy is heated to 600°C to 800°C, heated at a rate of 20°C / min to 100°C / min, kept at this temperature for 10 to 30 minutes, and then rapidly cooled to room temperature at a cooling rate of 10°C / min to 50°C / min.
[0025] 3. Isothermal aging treatment:
[0026] The alloy after the preliminary heat treatment is heated to 300°C-500°C at a rate of 5°C / min-10°C / min and kept at this temperature for 6 to 12 hours, and then cooled to room temperature at a rate of 10°C / min-20°C / min.
[0027] 4. Rolling process: proceed in the following order:
[0028] Multiple hot rolling:
[0029] The first stage of hot rolling: heat the alloy after strain induction treatment to 700℃-750℃, keep it warm for 20 minutes-30 minutes, and then hot roll it, with the deformation controlled at 30%-40%. Cool it to 300℃-500℃, and then immediately heat it to 600℃-750℃ again, keep it warm for 10-30 minutes, and then hot roll it for the second time, with the deformation controlled at 10%-30%; then cool it to room temperature.
[0030] Second stage hot rolling: heat the alloy after the first hot rolling to 600℃-650℃, keep it warm for 20 minutes-30 minutes, and then carry out the third hot rolling, with the deformation controlled at 30%-50%. Cool to 350℃-450℃, and immediately heat it again to 600℃-700℃, keep it warm for 10-30 minutes, and then carry out the fourth hot rolling, with the deformation controlled at 10%-40%. Cool to room temperature.
[0031] Alternate cold rolling:
[0032] The first stage of cold rolling: the alloy after the second stage of hot rolling is cold rolled at room temperature, the deformation is controlled at 20%-30%, and then the cold rolled alloy is placed in a 200℃~300℃ environment for heat treatment, kept warm for 1 hour-2 hours, and then cooled to room temperature.
[0033] Second stage cold rolling: The alloy after the first stage cold rolling is rotated 90 degrees and cold rolled again at room temperature, with the deformation controlled at 20%-35%. The cold rolled alloy is then placed in a 300℃-350℃ environment for heat treatment, kept warm for 1 to 2 hours, and then air-cooled to room temperature.
[0034] The third stage of cold rolling: the alloy after the second stage of cold rolling is rotated 180 degrees and cold rolled again at room temperature, the deformation is controlled at 20%-40%, and then the cold rolled alloy is placed in a 300℃-400℃ environment for heat treatment, kept warm for 1 to 2 hours, and then air-cooled to room temperature.
[0035] Final cold rolling: The alloy after the third stage of cold rolling is subjected to final room temperature cold rolling, with the deformation amount controlled at 20%-45% to obtain a foil with a thickness of 0.01 mm to 0.2 mm.
[0036] 5. Multi-stage aging treatment:
[0037] The first stage: heat the alloy to 250℃~300℃, keep it at this temperature for 1 hour to 3 hours, and cool it to room temperature;
[0038] The second stage: heat the alloy to 300℃~400℃, keep it at this temperature for 1-2 hours, and cool it to room temperature;
[0039] The third stage: heat the alloy to 400℃~600℃, keep it at this temperature for 2-3 hours, and cool it to room temperature.
[0040] 6. Stress relief treatment:
[0041] The alloy after the multi-stage aging treatment is subjected to stress relief treatment, the temperature is controlled at 300°C to 350°C, kept at this temperature for 2 hours to 4 hours, and then cooled to room temperature.
[0042] 7. Strain Inducing Treatment:
[0043] A constant tensile stress (the applied stress is 50% of the material yield strength) is applied to the alloy after stress relief treatment, the stress application rate is 1MPa / s to 2MPa / s, and the alloy is kept at 350°C to 400°C for 1 to 2 hours, then the stress is released at a rate of 1MPa / s to 2MPa / s and cooled to room temperature.
[0044] 8. Stabilization treatment:
[0045] The foil after strain induction treatment is heated to 200-300°C, kept at this temperature for 1-2 hours, and then cooled to room temperature at a rate of 5-10°C / min to stabilize the microstructure of the alloy.
[0046] 9. Final room temperature aging treatment:
[0047] Place the alloy foil in a room temperature environment and keep it warm for 2 to 4 hours.
[0048] The present invention effectively improves the elastic properties of the titanium alloy foil through the above innovative heat treatment process and multi-stage rolling processing method, so that the elastic strain of the foil is greater than 1%, meeting the application requirements of elastic connection.
[0049] Principle of the invention:
[0050] The present invention proposes a composition design and multi-stage heat treatment method based on a complex multi-component titanium alloy system, aiming to accurately control the alloy microstructure and phase stability through systematic and iterative alloy composition optimization and multiple heat treatment and cold rolling technologies.
[0051] 1. Composition optimization: Conventional titanium alloy composition design methods cannot produce foils with excellent elastic properties. This technology calculates the alloy characteristic parameter (η), considers the atomic percentage and number of valence electrons of each element, and ensures that the characteristic parameter (η) is lower than 4.20, thereby optimizing the alloy composition and ensuring phase stability.
[0052] 2. Preliminary heat treatment and isothermal aging: Rapidly heat in the range of 600℃-800℃, cool to room temperature at a high cooling rate after heat preservation, and induce the formation of a fine and uniform initial phase structure. Then, isothermal aging treatment is performed in the range of 300℃-500℃. By controlling the aging time and temperature, the composition structure is refined and the high-temperature stability of the alloy is enhanced.
[0053] 3. Multi-stage rolling processing: Combining multiple hot rolling and cold rolling technologies, through two-stage hot rolling and alternating cold rolling, using the dislocation movement and grain orientation rearrangement effect in crystal plasticity theory, to ensure the mechanical properties and internal stress elimination of the alloy, and to ensure high flexibility and uniformity.
[0054] 4: Multi-stage aging treatment and stress relief: Through gradual heating and heat preservation from 250℃ to 600℃, the stable growth and precipitation hardening of multi-stage precipitation phases are achieved. Stress relief treatment improves the dimensional stability of the alloy through the stress relaxation effect.
[0055] 5. Strain induction and stabilization treatment: Apply constant tensile stress at 350℃~400℃, and slowly release the stress after heat preservation to optimize the microstructure. The final stabilization treatment is carried out by heat preservation at 200℃ and aging treatment at room temperature to ensure the stability and excellent performance of the alloy during use.
[0056] The method of the present invention achieves high strength, high flexibility and excellent fatigue resistance of titanium alloy through the combination of multiple innovative technologies, demonstrating breakthrough progress in alloy composition optimization and heat treatment technology.
[0057] Advantages of the present invention:
[0058] Through innovative composition optimization technology, by using characteristic parameters (η) to optimize the composition of titanium alloy, the alloy can have excellent elastic properties after being prepared into foil.
[0059] The invention adopts a staged heat treatment method, including preliminary heat treatment, isothermal aging treatment and multi-stage aging treatment, to accurately control the temperature and time of each stage and improve the microstructural stability of the alloy.
[0060] Combining multiple hot rolling and cold rolling processes, using alternating cold rolling and rotation processing technology, by controlling the deformation amount and heat treatment temperature, the grain structure and dislocation distribution of the alloy are optimized, and the internal stress elimination effect is significantly improved.
[0061] The elastic properties of the titanium alloy materials obtained through this scheme are all improved, and the elastic recoverable strain is increased from 0.6% of conventional titanium alloys to more than 1.1%, an increase of more than 80%, which can meet the strict requirements of foils in different environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 Schematic diagram of the process of the present invention. DETAILED DESCRIPTION
[0063] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. Figure 1 shown.
[0064] Example 1
[0065] The alloy contains Ti, Nb, Zr and Sn elements, and the atomic percentage of the alloy elements is adjusted to Ti: 78%, Nb: 15%, Zr: 3%, Sn: 4%, so that the characteristic parameter (η) of the alloy satisfies: η = 4.15; the alloy is heated to 600°C, heated at a rate of 20°C / min, kept warm for 10 minutes, and then quickly cooled to room temperature at a cooling rate of 10°C / min; the alloy after preliminary heat treatment is heated to 300°C at a rate of 5°C / min and kept warm for 6 hours, and then cooled to room temperature at a rate of 10°C / min. Multiple hot rolling: the first stage hot rolling: the alloy after strain induction treatment is heated to 700°C, kept warm for 20 minutes, and hot rolled, and the deformation is controlled at 30%. Cool to 300°C, immediately heat to 600°C again, keep warm for 10 minutes, and perform a second hot rolling, and the deformation is controlled at 10%; cool to room temperature. Second stage hot rolling: heat the alloy after the first hot rolling to 600℃ and keep it warm for 20 minutes; perform the third hot rolling with the deformation controlled at 30%. Cool to 350℃, immediately heat to 600℃ again, keep it warm for 10 minutes, perform the fourth hot rolling with the deformation controlled at 10%. Cool to room temperature. Alternating cold rolling: first stage cold rolling: the alloy after the second stage hot rolling is cold rolled at room temperature, the deformation is controlled at 20%, and then the cold rolled alloy is placed in a 200°C environment for heat treatment, kept warm for 1 hour, and then cooled to room temperature; second stage cold rolling: the alloy after the first stage cold rolling is rotated 90 degrees, cold rolled again at room temperature, the deformation is controlled at 20%, and then the cold rolled alloy is placed in a 300°C environment for heat treatment, kept warm for 1 hour, and then air cooled to room temperature; third stage cold rolling: the alloy after the second stage cold rolling is rotated 180 degrees, cold rolled again at room temperature, the deformation is controlled at 20%, and then the cold rolled alloy is placed in a 300°C environment for heat treatment, kept warm for 1 hour, and then air cooled to room temperature; final cold rolling: the alloy after the third stage cold rolling is finally cold rolled at room temperature, the deformation is controlled at 20%, and a foil with a thickness of 0.01 mm is obtained. Multi-stage aging treatment: First stage: heat the alloy to 250℃, keep it warm for 1 hour, and cool it to room temperature; second stage: heat the alloy to 300℃, keep it warm for 1 hour, and cool it to room temperature; third stage: heat the alloy to 400℃, keep it warm for 2 hours, and cool it to room temperature. Stress relief treatment: The alloy after multi-stage aging treatment is subjected to stress relief treatment, the temperature is controlled at 300℃, kept warm for 2 hours, and then cooled to room temperature. Strain induction treatment: a constant tensile stress (stress is 50% of the yield strength of the material) is applied to the alloy after stress relief treatment, the stress application rate is 1MPa / s, and it is kept warm in a 350℃ environment for 1 hour, then the stress is released at a rate of 1MPa / s, and cooled to room temperature. Stabilization treatment: the foil after strain induction treatment is heated to 200℃, kept warm for 1 hour, and then cooled to room temperature at a rate of 5℃ / min to stabilize the microstructure of the alloy.Final room temperature aging treatment: place the alloy foil in a room temperature environment and keep it warm for 2 hours.
[0066] In this embodiment, the foil material prepared by the above-mentioned heat treatment process and multi-stage rolling processing method has an elastic strain of 1.2%.
[0067] Example 2
[0068] The alloy contains Ti, V, Al and Mo elements, and the atomic percentage of the alloy elements is adjusted to Ti: 78%, V: 12%, Al: 5%, Mo: 5%, so that the characteristic parameter (η) of the alloy satisfies: η = 4.17; the alloy is heated to 800°C, heated at a rate of 100°C / min, kept warm for 30 minutes, and then quickly cooled to room temperature at a cooling rate of 50°C / min; the alloy after preliminary heat treatment is heated to 500°C at a rate of 10°C / min and kept warm for 12 hours, and then cooled to room temperature at a rate of 20°C / min. Multiple hot rolling: the first stage hot rolling: the alloy after strain induction treatment is heated to 750°C, kept warm for 30 minutes, and hot rolled, and the deformation is controlled at 40%. Cool to 500°C, immediately heat to 750°C again, keep warm for 30 minutes, and perform a second hot rolling, and the deformation is controlled at 30%; cool to room temperature. Second stage hot rolling: heat the alloy after the first hot rolling to 650℃, keep it warm for 30 minutes, and then carry out the third hot rolling, with the deformation controlled at 50%. Cool to 450℃, and immediately heat to 700℃ again, keep it warm for 30 minutes, and then carry out the fourth hot rolling, with the deformation controlled at 40%. Cool to room temperature. Alternating cold rolling: first stage cold rolling: the alloy after the second stage hot rolling is cold rolled at room temperature, the deformation is controlled at 30%, and then the cold rolled alloy is placed in a 300°C environment for heat treatment, kept warm for 2 hours, and then cooled to room temperature; second stage cold rolling: the alloy after the first stage cold rolling is rotated 90 degrees, cold rolled again at room temperature, the deformation is controlled at 35%, and then the cold rolled alloy is placed in a 350°C environment for heat treatment, kept warm for 2 hours, and then air cooled to room temperature; third stage cold rolling: the alloy after the second stage cold rolling is rotated 180 degrees, cold rolled again at room temperature, the deformation is controlled at 40%, and then the cold rolled alloy is placed in a 400°C environment for heat treatment, kept warm for 2 hours, and then air cooled to room temperature; final cold rolling: the alloy after the third stage cold rolling is finally cold rolled at room temperature, the deformation is controlled at 45%, and a foil with a thickness of 0.2 mm is obtained. Multi-stage aging treatment: First stage: heat the alloy to 300℃, keep it warm for 3 hours, and cool it to room temperature; second stage: heat the alloy to 400℃, keep it warm for 2 hours, and cool it to room temperature; third stage: heat the alloy to 600℃, keep it warm for 3 hours, and cool it to room temperature. Stress relief treatment: The alloy after multi-stage aging treatment is subjected to stress relief treatment, the temperature is controlled at 350℃, kept warm for 4 hours, and then cooled to room temperature. Strain induction treatment: a constant tensile stress (stress is 50% of the yield strength of the material) is applied to the alloy after stress relief treatment, the stress application rate is 2MPa / s, and it is kept warm in a 400℃ environment for 2 hours, then the stress is released at a rate of 2MPa / s, and cooled to room temperature. Stabilization treatment: the foil after strain induction treatment is heated to 300℃, kept warm for 2 hours, and then cooled to room temperature at a rate of 10℃ / min to stabilize the microstructure of the alloy.Final room temperature aging treatment: place the alloy foil in a room temperature environment and keep it warm for 4 hours.
[0069] In this embodiment, the elastic strain of the foil obtained by the above-mentioned heat treatment process and multi-stage rolling processing method is 1.3%.
[0070] Example 3
[0071] The alloy contains Ti, Fe, and Mn elements, and the atomic percentage of the alloy element composition is adjusted to Ti: 95%, Fe: 2%, and Mn: 3%, so that the characteristic parameter (η) of the alloy satisfies: η=4.17; the alloy is heated to 700°C, heated at a rate of 60°C / min, kept warm for 20 minutes, and then quickly cooled to room temperature at a cooling rate of 30°C / min; the alloy after preliminary heat treatment is heated to 400°C at a rate of 5°C / min to 10°C / min and kept warm for 8 hours, and then cooled to room temperature at a rate of 15°C / min. Multiple hot rolling: First stage hot rolling: the alloy after strain induction treatment is heated to 725°C, kept warm for 25 minutes, and hot rolled, and the deformation is controlled at 35%. Cool to 400°C, immediately heat to 700°C again, keep warm for 15 minutes, and perform a second hot rolling, and the deformation is controlled at 20%; cool to room temperature. Second stage hot rolling: heat the alloy after the first hot rolling to 625℃, keep it warm for 25 minutes, and then carry out the third hot rolling, with the deformation controlled at 40%. Cool to 400℃, and immediately heat to 650℃ again, keep it warm for 20 minutes, and then carry out the fourth hot rolling, with the deformation controlled at 25%. Cool to room temperature. Alternating cold rolling: first stage cold rolling: the alloy after the second stage hot rolling is cold rolled at room temperature, the deformation is controlled at 25%, and then the cold rolled alloy is placed in a 250°C environment for heat treatment, kept warm for 1.5 hours, and then cooled to room temperature; second stage cold rolling: the alloy after the first stage cold rolling is rotated 90 degrees, cold rolled again at room temperature, the deformation is controlled at 30%, and then the cold rolled alloy is placed in a 325°C environment for heat treatment, kept warm for 1.5 hours, and then air cooled to room temperature; third stage cold rolling: the alloy after the second stage cold rolling is rotated 180 degrees, cold rolled again at room temperature, the deformation is controlled at 30%, and then the cold rolled alloy is placed in a 350°C environment for heat treatment, kept warm for 1.5 hours, and then air cooled to room temperature; final cold rolling: the alloy after the third stage cold rolling is finally cold rolled at room temperature, the deformation is controlled at 30%, and a foil with a thickness of 0.05 mm is obtained. Multi-stage aging treatment: First stage: heat the alloy to 275℃, keep it warm for 2 hours, and cool it to room temperature; Second stage: heat the alloy to 350℃, keep it warm for 1.5 hours, and cool it to room temperature; Third stage: heat the alloy to 500℃, keep it warm for 2.5 hours, and cool it to room temperature. Stress relief treatment: The alloy after multi-stage aging treatment is subjected to stress relief treatment, the temperature is controlled at 325℃, kept warm for 3 hours, and then cooled to room temperature. Strain induction treatment: apply a constant tensile stress (stress is 50% of the material yield strength) to the alloy after stress relief treatment, the stress application rate is 1.5MPa / s, keep it warm in a 375℃ environment for 1.5 hours, then release the stress at a rate of 1.5MPa / s, and cool it to room temperature.Stabilization treatment: Heat the foil after strain induction treatment to 250°C, keep it warm for 1.5 hours, and then cool it to room temperature at a rate of 7.5°C / min to stabilize the microstructure of the alloy. Final room temperature aging treatment: Place the alloy foil in a room temperature environment and keep it warm for 3 hours.
[0072] In this embodiment, the elastic strain of the foil obtained by the above-mentioned heat treatment process and multi-stage rolling processing method is 1.1%.
[0073] Example 4
[0074] The alloy contains Ti, Ta, and Cr elements, and the atomic percentage of the alloy elements is adjusted to Ti: 83%, Ta: 14%, and Cr: 3%, so that the characteristic parameter (η) of the alloy satisfies: η = 4.2; the alloy is heated to 600°C, heated at a rate of 75°C / min, kept warm for 15 minutes, and then quickly cooled to room temperature at a cooling rate of 15°C / min; the alloy after preliminary heat treatment is heated to 300°C at a rate of 6°C / min and kept warm for 7 hours, and then cooled to room temperature at a rate of 12.5°C / min. Multiple hot rolling: First stage hot rolling: The alloy after strain induction treatment is heated to 725°C, kept warm for 25 minutes, and hot rolled, and the deformation is controlled at 35%. Cool to 450°C, immediately heat to 620°C again, keep warm for 20 minutes, and perform a second hot rolling, and the deformation is controlled at 25%; cool to room temperature. Second stage hot rolling: heat the alloy after the first hot rolling to 620℃, keep it warm for 25 minutes, and then carry out the third hot rolling, with the deformation controlled at 40%. Cool it to 420℃, and then immediately heat it again to 630℃, keep it warm for 20 minutes, and then carry out the fourth hot rolling, with the deformation controlled at 15%. Cool it to room temperature. Alternating cold rolling: first stage cold rolling: the alloy after the second stage hot rolling is cold rolled at room temperature, the deformation is controlled at 25%, and then the cold rolled alloy is placed in a 250°C environment for heat treatment, kept warm for 1.8 hours, and then cooled to room temperature; second stage cold rolling: the alloy after the first stage cold rolling is rotated 90 degrees, cold rolled again at room temperature, the deformation is controlled at 30%, and then the cold rolled alloy is placed in a 321°C environment for heat treatment, kept warm for 1.4 hours, and then air cooled to room temperature; third stage cold rolling: the alloy after the second stage cold rolling is rotated 180 degrees, cold rolled again at room temperature, the deformation is controlled at 36%, and then the cold rolled alloy is placed in a 360°C environment for heat treatment, kept warm for 1.4 hours, and then air cooled to room temperature; final cold rolling: the alloy after the third stage cold rolling is finally cold rolled at room temperature, the deformation is controlled at 35%, and a foil with a thickness of 0.17 mm is obtained. Multi-stage aging treatment: Stage 1: Heat the alloy to 270°C, keep it warm for 2 hours, and cool it to room temperature; Stage 2: Heat the alloy to 350°C, keep it warm for 1.4 hours, and cool it to room temperature; Stage 3: Heat the alloy to 500°C, keep it warm for 2.6 hours, and cool it to room temperature. Stress relief treatment: The alloy after multi-stage aging treatment is subjected to stress relief treatment, the temperature is controlled at 340°C, kept warm for 3 hours, and then cooled to room temperature. Strain induction treatment: Apply a constant tensile stress (stress is 50% of the material yield strength) to the alloy after stress relief treatment, the stress application rate is 1.4MPa / s, keep it warm in a 380°C environment for 1.2 hours, then release the stress at a rate of 1.4MPa / s, and cool it to room temperature.Stabilization treatment: Heat the foil after strain induction treatment to 270°C, keep it warm for 2 hours, and then cool it to room temperature at a rate of 8°C / min to stabilize the microstructure of the alloy. Final room temperature aging treatment: Place the alloy foil in a room temperature environment and keep it warm for 3 hours.
[0075] In this embodiment, the elastic strain of the foil obtained by the above-mentioned heat treatment process and multi-stage rolling processing method is 1.2%.
[0076] Example 5
[0077] The alloy contains Ti, Nb, Zr and Sn elements, and the atomic percentage of the alloy elements is adjusted to Ti: 73%, Nb: 16%, Zr: 3%, Sn: 8%, so that the characteristic parameter (η) of the alloy satisfies: η = 4.16; the alloy is heated to 650°C, heated at a rate of 90°C / min, kept at this temperature for 25 minutes, and then quickly cooled to room temperature at a cooling rate of 15°C / min; the alloy after the preliminary heat treatment is heated to 350°C at a rate of 6°C / min and kept at this temperature for 7 hours, and then cooled to room temperature at a rate of 17.5°C / min. Multiple hot rolling: the first stage hot rolling: the alloy after the strain induction treatment is heated to 720°C, kept at this temperature for 28 minutes, and hot rolled, and the deformation is controlled at 32%. Cool to 320°C, immediately heat to 680°C again, keep at this temperature for 17 minutes, and carry out the second hot rolling, and the deformation is controlled at 12%; cool to room temperature. Second stage hot rolling: heat the alloy after the first hot rolling to 610℃, keep it warm for 22 minutes, and then carry out the third hot rolling, with the deformation controlled at 32%. Cool to 370℃, immediately heat to 610℃ again, keep it warm for 20 minutes, and then carry out the fourth hot rolling, with the deformation controlled at 15%. Cool to room temperature. Alternating cold rolling: first stage cold rolling: the alloy after the second stage hot rolling is cold rolled at room temperature, the deformation is controlled at 28%, and then the cold rolled alloy is placed in a 220°C environment for heat treatment, kept warm for 1.2 hours, and then cooled to room temperature; second stage cold rolling: the alloy after the first stage cold rolling is rotated 90 degrees, cold rolled again at room temperature, the deformation is controlled at 30%, and then the cold rolled alloy is placed in a 310°C environment for heat treatment, kept warm for 1.2 hours, and then air cooled to room temperature; third stage cold rolling: the alloy after the second stage cold rolling is rotated 180 degrees, cold rolled again at room temperature, the deformation is controlled at 35%, and then the cold rolled alloy is placed in a 310°C environment for heat treatment, kept warm for 1.4 hours, and then air cooled to room temperature; final cold rolling: the alloy after the third stage cold rolling is finally cold rolled at room temperature, the deformation is controlled at 35%, and a foil with a thickness of 0.15 mm is obtained. Multi-stage aging treatment: First stage: heat the alloy to 280℃, keep it warm for 2.5 hours, and cool it to room temperature; Second stage: heat the alloy to 350℃, keep it warm for 1.6 hours, and cool it to room temperature; Third stage: heat the alloy to 550℃, keep it warm for 2.1 hours, and cool it to room temperature. Stress relief treatment: The alloy after multi-stage aging treatment is subjected to stress relief treatment, the temperature is controlled at 330℃, kept warm for 2.5 hours, and then cooled to room temperature. Strain induction treatment: apply a constant tensile stress (stress is 50% of the material yield strength) to the alloy after stress relief treatment, the stress application rate is 2MPa / s, keep it warm in a 360℃ environment for 1 hour, then release the stress at a rate of 1MPa / s, and cool it to room temperature.Stabilization treatment: Heat the strain-induced treated foil to 200°C, keep it warm for 1.5 hours, and then cool it to room temperature at a rate of 6°C / min to stabilize the microstructure of the alloy. Final room temperature aging treatment: Place the alloy foil in a room temperature environment and keep it warm for 3.5 hours.
[0078] In this embodiment, the elastic strain of the foil obtained by the above-mentioned heat treatment process and multi-stage rolling processing method is 1.5%.
Claims
1. A method for improving the elastic properties of titanium alloy foil, characterized in that: The following steps are involved: Step 1. Alloy composition optimization: adjust the content of alloy elements so that the characteristic parameter η of the alloy satisfies: 4.14≤η≤4.20; Step 2. Preliminary heat treatment: heating the alloy at a certain rate, keeping the temperature and then cooling it rapidly to room temperature; Step 3. Isothermal aging treatment: the alloy after the preliminary heat treatment is heated up and then kept warm, and then cooled to room temperature at a certain speed; Step 4. Rolling process: the alloy is subjected to multiple hot rolling, alternating cold rolling and final cold rolling in sequence to obtain a foil; wherein the hot rolling includes two stages and the alternating cold rolling includes three stages; Step 5. Multi-stage aging treatment: subject the foil to three-stage aging treatment; Step 6. Stress relief treatment: The alloy after multi-stage aging treatment is kept at 300°C to 350°C for 2h to 4h, and then cooled to room temperature for stress relief treatment; Step 7. Strain induction treatment: applying a constant tensile stress to the stress-relieved alloy, releasing the stress after heat preservation at high temperature, and then cooling to room temperature; Step 8. Stabilization treatment: The foil after strain induction treatment is heated, kept warm, and then cooled to room temperature to stabilize the microstructure of the alloy; Step 9. Final room temperature aging treatment: placing the alloy foil at room temperature for 2 hours to 4 hours to obtain a titanium alloy foil with an elastic strain greater than 1%.
2. A method for improving the elastic properties of titanium alloy foil according to claim 1, characterized in that: In step 1, the calculation method of the alloy characteristic parameters is: a. Calculate the atomic percentage of each element in the titanium alloy, including but not limited to: Ti, V, Al, Mo, Zr, Sn, Nb, Fe, Mn, Ta and Cr; b. Calculate the electron concentration of each element based on the atomic percentage and the number of valence electrons of each element by multiplying the atomic percentage of the element by the number of valence electrons of the element; where the number of valence electrons of each element is as follows: Ti 4, V 5, Al 3, Mo 6, Zr 4, Sn 4, Nb 5, Fe 8, Mn 7, Ta 5 and Cr 6; c. Add the electron concentrations of all elements to obtain the characteristic parameter η.
3. The method for improving the elastic properties of titanium alloy foil according to claim 1, characterized in that: In step 2, the heating rate is 20°C / min to 100°C / min to raise the temperature to 600°C to 800°C, and the holding time is 10min to 30min; the cooling rate of rapid cooling is 10°C / min to 50°C / min.
4. The method for improving the elastic properties of titanium alloy foil according to claim 1, characterized in that: In step 3, the alloy is heated to 300°C to 500°C at a rate of 5°C / min to 10°C / min, and the holding time is 6h to 12h; The cooling rate of rapid cooling is 10°C / min to 50°C / min.
5. The method for improving the elastic properties of titanium alloy foil according to claim 1, characterized in that: In step 4, in the multiple hot rolling, the first stage hot rolling process is: heating the alloy after strain induction treatment to 700°C to 750°C, keeping it warm for 20min to 30min, and hot rolling, and the deformation is controlled at 30% to 40%; cooling to 300°C to 500°C, immediately heating it again to 600°C to 750°C, keeping it warm for 10min to 30min, and hot rolling it for the second time, and the deformation is controlled at 10% to 30%; cooling to room temperature; The second stage of hot rolling is as follows: heating the alloy after the first hot rolling to 600°C ~ 650°C, keeping it warm for 20min ~ 30min, performing the third hot rolling, and controlling the deformation amount within 30% ~ 50%; cooling to 350°C ~ 450°C, immediately heating it again to 600°C ~ 700°C, keeping it warm for 10min ~ 30min, performing the fourth hot rolling, and controlling the deformation amount within 10% ~ 40%; cooling to room temperature.
6. The method for improving the elastic properties of titanium alloy foil according to claim 1, characterized in that: In step 4, in the alternating cold rolling, the first stage of cold rolling is to cold roll the alloy after the second stage of hot rolling at room temperature, and control the deformation amount to 20% to 30%, and then place the cold rolled alloy in an environment of 200° C. to 300° C. for heat treatment, keep the temperature for 1 h to 2 h, and then cool to room temperature; Second stage cold rolling: the alloy after the first stage cold rolling is rotated 90 degrees and cold rolled again at room temperature, the deformation is controlled at 20% to 35%, and then the cold rolled alloy is placed in a 300℃ to 350℃ environment for heat treatment, kept at this temperature for 1h to 2h, and then air-cooled to room temperature; The third stage of cold rolling: the alloy after the second stage of cold rolling is rotated 180 degrees and cold rolled again at room temperature, the deformation is controlled at 20% to 40%, and then the cold rolled alloy is placed in a 300°C to 400°C environment for heat treatment, kept warm for 1h to 2h, and then air-cooled to room temperature.
7. The method for improving the elastic properties of titanium alloy foil according to claim 1, characterized in that: In step 4, the final cold rolling process is: the alloy after the third stage of cold rolling is subjected to final room temperature cold rolling, and the deformation is controlled at 20% to 45%, so as to obtain a foil with a thickness of 0.01 mm to 0.2 mm.
8. The method for improving the elastic properties of titanium alloy foil according to claim 1, characterized in that: In step 5, the three-stage aging process is as follows: The first stage: heat the alloy to 250℃~300℃, keep it warm for 1h~3h, and cool it to room temperature; The second stage: heat the alloy to 300℃~400℃, keep it warm for 1h~2h, and cool it to room temperature; The third stage: heat the alloy to 400℃~600℃, keep it warm for 2h~3h, and cool it to room temperature.
9. The method for improving the elastic properties of titanium alloy foil according to claim 1, characterized in that: In step 7, the tensile stress applied is 50% of the yield strength of the material; the stress application rate is 1 MPa / s to 2 MPa / s; the insulation temperature is 350°C to 400°C, and the insulation time is 1h to 2h; the stress release rate is 1 MPa / s to 2 MPa / s.