Metal piece surface machining treatment method and machining equipment thereof

By adding Cu components and SiO2 powder to CoCrFeMnNi high-entropy alloy powder, metal cermet powder was prepared, and thermal spraying technology was used to solve the shortcomings of CoCrFeMnNi high-entropy alloy powder in the prior art in terms of corrosion resistance and wear resistance, which significantly Improves the corrosion and wear resistance of metal parts and extends the service life.

CN118957479AInactive Publication Date: 2024-11-15GUANGZHOU HESHENG PRECISION MASCH EQUIP CO LTD

Patent Information

Application Number
CN202411030781.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing CoCrFeMnNi high-entropy alloy powders have defects in corrosion resistance and wear resistance, and it is difficult to meet high-demand application scenarios.

Method used

The CoCrFeCuMnNi high-entropy alloy powder was formed by adding Cu components, and combined with SiO2 powder was used to prepare a cermet powder, and a coating was formed on the surface of the stainless steel substrate using thermal spraying technology. The method includes smelting Fe, Cu, Co, Ni, Cr and Mn elements, using electrode-induced melting gas atomization method to produce high entropy alloy powder, and then processing with SiO2 powder and surfactant under hydrothermal conditions to form particle diameters Surface pretreatment and thermal spraying were performed in 1-30 μm of metal cermet powder.

Benefits of technology

It significantly improves the corrosion resistance and wear resistance of metal parts, extends the service life, and is suitable for high-demand application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957479A_ABST
    Figure CN118957479A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of ceramic metal coatings, and particularly discloses a metal part surface machining treatment method and machining equipment thereof. The treatment method comprises the step of thermally spraying metal ceramic powder on a stainless steel base material, the metal ceramic powder is prepared from the following raw materials in parts by weight: 100 parts of CoCrFeCuMnNi high-entropy alloy powder, 20 to 30 parts of SiO2 powder, 10 to 20 parts of a surfactant and 5 to 10 parts of urea, according to the method, the mixture of the CoCrFeCuMnNi high-entropy alloy powder and the SiO powder is subjected to thermal spraying, the ceramic metal coating formed on the stainless steel base material has excellent wear resistance and corrosion resistance, the service life of a metal piece can be remarkably prolonged through the coating, and the method is particularly suitable for application scenes with high requirements for wear resistance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of ceramic metal coatings, and specifically discloses a metal part surface processing method and processing equipment thereof. Background Art

[0002] Anti-corrosion is the process of protecting metal objects that are prone to rust by taking various measures to extend their service life. Chemical anti-corrosion, physical anti-corrosion, electrochemical anti-corrosion and other methods are usually used.

[0003] The chemical, electrochemical or physical reaction between metal and the environment in which it is located causes the deterioration and deterioration of metal, which is called metal corrosion. Corrosion is a very common phenomenon. From the point of view of thermodynamics, except for a very small number of precious metals (Au, Pt, etc.), the corrosion of general metals is a spontaneous process. People have realized that the metals used are rarely damaged by simple mechanical factors (such as tension, compression, impact, fatigue, fracture and wear, etc.) or other physical factors (such as heat energy, light energy, etc.). The damage of most metal materials is related to their corrosion factors. Therefore, the corrosion of metal materials has become an important issue that cannot be ignored today.

[0004] The existing technologies for high entropy alloy powder spraying anti-corrosion mainly include the following:

[0005] 1. Laser cladding technology

[0006] Technical principle: Add protective material to the surface of the substrate, irradiate with high-energy laser beam to make the substrate and protective material co-melt, then quickly cool and solidify to form a coating with surface modification.

[0007] Advantages: high power density, low heat input, little effect on the substrate, fast heating and cooling, close bonding between the coating and the substrate, fine coating grains and low segregation of elemental components in the coating.

[0008] Application examples: Xu et al. used laser cladding technology to prepare CoCrFeNiTiAlx (x=0, 0.5%, 1.0%, 1.5%, 2.0%) high entropy alloy coating on the surface of AISI1045 steel; Zhang et al. used laser cladding technology to prepare AlCoCrFeNiSi high entropy alloy coating on the surface of AISI 304 stainless steel.

[0009] 2. Thermal spraying technology

[0010] Technical principle: The heat generated by the heat source is used to heat the coating material to a molten state, and then a high-speed airflow is used to atomize the molten coating material into fine particles, and the fine particles are sprayed onto the surface of the substrate with the help of external thrust to form a coating.

[0011] Advantages: There is almost no limit to the materials that can be sprayed, from high entropy alloys to high entropy ceramic coatings.

[0012] Specific methods: including atmospheric plasma spraying, etc. The coatings prepared by atmospheric plasma spraying are mostly layered structures, but the performance of the coatings can be further improved by combining with appropriate heat treatment processes.

[0013] Application example: The CoCrFeMo0.85Ni high entropy alloy coating prepared by Fanicchia et al. on carbon steel by thermal spraying technology showed better corrosion resistance than the substrate in 3.5wt% NaCl solution.

[0014] 3. Cold spray technology

[0015] Technical principle: Metal particles (1-50μm) collide with the substrate surface at supersonic speed and firmly adhere to the substrate surface to form a coating. The whole process is carried out at a relatively low temperature and the metal particles are not melted.

[0016] Advantages: There is basically no phase change or oxidation during the powder deposition process, and it can be used to prepare thick coatings with low porosity.

[0017] Application example: Anupam et al. successfully prepared AlCoCrFeNi coating on the surface of Ni-based alloy by cold spraying technology. After oxidation at 1100℃ for 25h, the coating can still protect the substrate.

[0018] In the thermal spraying technology of the prior art, most cases use CoCrFeMnNi high entropy alloy powder as a material for spraying protection on the surface of metal parts. The above-mentioned CoCrFeMnNi high entropy alloy powder still has defects in corrosion resistance and wear resistance, and further improvements are needed. Summary of the invention

[0019] In order to solve the above problems, the present invention discloses a metal part surface processing method and processing equipment.

[0020] The technical solution of the present invention is as follows:

[0021] A metal part surface processing method includes the steps of thermally spraying metal ceramic powder on a stainless steel substrate;

[0022] The metal ceramic powder is composed of the following raw materials by weight:

[0023]

[0024] Furthermore, in the above-mentioned metal part surface processing method, the CoCrFeCuMnNi high entropy alloy powder is prepared by the following steps:

[0025] 1) Cut Fe, Cu, Co, Ni, Cr and Mn elemental small pieces into pieces no larger than 4 cm 3 Single-substance small pieces, and wash and dry them; when melting the above-mentioned single-substance small pieces, put Cu, Mn, Co, Fe, Ni and Cr element single-substance small pieces into a medium frequency induction furnace in the order of melting point from low to high; the parameters of the medium frequency induction furnace smelting are: slowly increase the induction furnace smelting power at a speed of 3-5kW / 5min, so that the smelting power reaches 35-40kW, and the smelting time is 3-6h, and CoCrFeCuMnNi alloy rods are obtained;

[0026] (2) The CoCrFeCuMnNi alloy rod is subjected to an electrode induction melting gas atomization method to obtain a CoCrFeCuMnNi high entropy alloy powder; the melting temperature in the electrode induction melting gas atomization method is maintained between 1650°C and 1680°C, the holding temperature is maintained between 1320°C and 1340°C, and the refining time is 5-10 minutes. Calculated by weight, the CoCrFeCuMnNi high entropy alloy powder includes:

[0027]

[0028] Furthermore, in the above-mentioned metal part surface processing method, the metal ceramic powder is prepared by the following steps: step 1, CoCrFeCuMnNi high entropy alloy powder, SiO 2 The powder and surfactant are put into an appropriate amount of deionized water and stirred for 1-2 hours under ultrasonic conditions to obtain suspension a.

[0029] Step 2: Add urea to suspension a and stir for 10 to 30 minutes to obtain suspension b.

[0030] Step 3: transfer the suspension b to a stainless steel autoclave and perform hydrothermal treatment at 140-180° C. for 2-6 h; then centrifuge at 10,000-15,000 rpm, remove the lower precipitate, and dry at 90-110° C. for 4-6 h to obtain a precursor powder.

[0031] Step 4: heat-treating the precursor powder in an inert gas atmosphere at 1400-1500° C. for 1-3 hours to obtain a metal ceramic powder.

[0032] Furthermore, in the above-mentioned metal part surface processing method, the particle size range of the metal ceramic powder is 1-30 μm.

[0033] Furthermore, the above-mentioned metal part surface processing method comprises the following steps:

[0034] (1) Surface pretreatment: Pretreat the surface of the stainless steel substrate to remove surface burrs and rust, so that the rust removal level of the stainless steel substrate surface is not less than Sa3.0;

[0035] (2) Thermal spraying: placing the metal ceramic powder into a thermal spraying system, and thermally spraying the metal powder onto the surface of the stainless steel substrate to form a coating.

[0036] Furthermore, in the above-mentioned metal part surface processing method, the step (2) thermal spraying uses a metal powder spraying torch to spray: comprising the following steps:

[0037] (21) Use an oxyacetylene flame to heat the surface of the stainless steel substrate to about 400-500°C, then keep the nozzle 120-150mm away from the surface of the stainless steel substrate, spray the metal ceramic powder evenly on the surface of the workpiece, and then melt it with the flame until the surface has a mirror reflection, and then gradually move the melting position to make the alloy powder and the stainless steel substrate melt and diffuse with each other to form a strong bonding layer.

[0038] The invention also discloses a processing device used for the above-mentioned metal part surface processing method.

[0039] Preferably, the above-mentioned processing equipment includes a workbench, a metal powder spraying welding torch, a lifting mechanism, a base, a power supply mechanism and a walking mechanism; the workbench is a rectangular plane workbench, a storage rack is provided on the other side of the workbench, and a clamping device is provided on the periphery of the storage rack; the workbench is installed as a whole on the base; the metal powder spraying welding torch is provided on one side of the workbench, and a lifting mechanism is installed below the metal powder spraying welding torch; the lifting mechanism is installed on the base; the base is hollow, in which a power supply mechanism is provided; a walking mechanism is provided below the base.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] The invention discloses a metal part surface processing method and a processing device thereof. The invention improves the existing CoCrFeMnNi high entropy alloy powder, adds a specific content of Cu component therein, forms CoCrFeCuMnNi high entropy alloy powder, and further adds SiO 2 The powder is made into a metal ceramic powder. It is found that when the metal ceramic powder is used for thermal spraying, it is better than the CoCrFeMnNi high entropy alloy powder without adding Cu component and the CoCrFeMnNi high entropy alloy powder without adding SiO 2 The corrosion resistance and wear resistance of the powder are greatly increased, which can significantly extend the service life of metal parts. It is particularly suitable for application scenarios with high requirements for wear resistance and corrosion resistance. At the same time, the present invention also discloses equipment that can conveniently use the above method to process the surface of metal parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 A schematic diagram of the processing equipment according to the present invention;

[0043] Figure 2 is the time (h) when corrosion begins to occur in the neutral salt spray test, data of Examples 1-3 and Comparative Examples 1-3;

[0044] Figure 3 is the concentration of iron ions in acidic immersion (μg / mL), data of Examples 1-3 and Comparative Examples 1-3;

[0045] Figure 4 is the impact resistance (kg.cm), data of Examples 1-3 and Comparative Examples 1-3;

[0046] Figure 5 is the friction coefficient, data of Examples 1-3 and Comparative Examples 1-3. DETAILED DESCRIPTION

[0047] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] A metal part surface processing method includes the steps of thermally spraying metal ceramic powder on a stainless steel substrate;

[0049] The metal ceramic powder is composed of the following raw materials by weight:

[0050]

[0051] The CoCrFeCuMnNi high entropy alloy powder is prepared by the following steps:

[0052] 1) Cut Fe, Cu, Co, Ni, Cr and Mn elemental small pieces into pieces no larger than 4 cm 3 Single-substance small pieces, and wash and dry them; when melting the above-mentioned single-substance small pieces, put Cu, Mn, Co, Fe, Ni and Cr element single-substance small pieces into a medium frequency induction furnace in the order of melting point from low to high; the parameters of the medium frequency induction furnace smelting are: slowly increase the induction furnace smelting power at a speed of 3-5kW / 5min, so that the smelting power reaches 35-40kW, and the smelting time is 3-6h, and CoCrFeCuMnNi alloy rods are obtained;

[0053] (2) The CoCrFeCuMnNi alloy rod is subjected to an electrode induction melting gas atomization method to obtain a CoCrFeCuMnNi high entropy alloy powder; the melting temperature in the electrode induction melting gas atomization method is maintained between 1650°C and 1680°C, the holding temperature is maintained between 1320°C and 1340°C, and the refining time is 5-10min.

[0054] In the CoCrFeCuMnNi high entropy alloy powder,

[0055]

[0056] The metal ceramic powder is prepared by the following steps:

[0057] Step 1: CoCrFeCuMnNi high entropy alloy powder, SiO 2 The powder and surfactant are put into an appropriate amount of deionized water and stirred for 1-2 hours under ultrasonic conditions to obtain suspension a.

[0058] Step 2: Add urea to suspension a and stir for 10 to 30 minutes to obtain suspension b.

[0059] Step 3: transfer the suspension b to a stainless steel autoclave and perform hydrothermal treatment at 140-180° C. for 2-6 h; then centrifuge at 10,000-15,000 rpm, remove the lower precipitate, and dry at 90-110° C. for 4-6 h to obtain a precursor powder.

[0060] Step 4: heat-treating the precursor powder in an inert gas atmosphere at 1400-1500° C. for 1-3 hours to obtain a metal ceramic powder.

[0061] The surfactant is fatty acid diglyceride.

[0062] Example 1

[0063] A metal part surface processing method includes the steps of thermally spraying metal ceramic powder on a stainless steel substrate;

[0064] The metal ceramic powder is composed of the following raw materials by weight:

[0065]

[0066] The CoCrFeCuMnNi high entropy alloy powder is prepared by the following steps:

[0067] 1) Cut Fe, Cu, Co, Ni, Cr and Mn elemental small pieces into pieces no larger than 4 cm 3Single-substance small pieces, and wash and dry them; when melting the above-mentioned single-substance small pieces, put Cu, Mn, Co, Fe, Ni and Cr element single-substance small pieces into a medium frequency induction furnace in the order of melting point from low to high; the parameters of the medium frequency induction furnace smelting are: slowly increase the induction furnace smelting power at a speed of 3-5kW / 5min, so that the smelting power reaches 35-40kW, and the smelting time is 3-6h, and CoCrFeCuMnNi alloy rods are obtained;

[0068] (2) The CoCrFeCuMnNi alloy rod is subjected to an electrode induction melting gas atomization method to obtain a CoCrFeCuMnNi high entropy alloy powder; the melting temperature in the electrode induction melting gas atomization method is maintained between 1650°C and 1680°C, the holding temperature is maintained between 1320°C and 1340°C, and the refining time is 5-10min.

[0069] In the CoCrFeCuMnNi high entropy alloy powder,

[0070]

[0071] The metal ceramic powder is prepared by the following steps:

[0072] Step 1: CoCrFeCuMnNi high entropy alloy powder, SiO 2 The powder and surfactant are put into an appropriate amount of deionized water and stirred for 1-2 hours under ultrasonic conditions to obtain suspension a.

[0073] Step 2: Add urea to suspension a and stir for 10 to 30 minutes to obtain suspension b.

[0074] Step 3: transfer the suspension b to a stainless steel autoclave and perform hydrothermal treatment at 140-180° C. for 2-6 h; then centrifuge at 10,000-15,000 rpm, remove the lower precipitate, and dry at 90-110° C. for 4-6 h to obtain a precursor powder.

[0075] Step 4: heat-treating the precursor powder in an inert gas atmosphere at 1400-1500° C. for 1-3 hours to obtain a metal ceramic powder.

[0076] Example 2

[0077] A metal part surface processing method includes the steps of thermally spraying metal ceramic powder on a stainless steel substrate;

[0078] The metal ceramic powder is composed of the following raw materials by weight:

[0079]

[0080] The CoCrFeCuMnNi high entropy alloy powder is prepared by the following steps:

[0081] 1) Cut Fe, Cu, Co, Ni, Cr and Mn elemental small pieces into pieces no larger than 4 cm 3 Single-substance small pieces, and wash and dry them; when melting the above-mentioned single-substance small pieces, put Cu, Mn, Co, Fe, Ni and Cr element single-substance small pieces into a medium frequency induction furnace in the order of melting point from low to high; the parameters of the medium frequency induction furnace smelting are: slowly increase the induction furnace smelting power at a speed of 3-5kW / 5min, so that the smelting power reaches 35-40kW, and the smelting time is 3-6h, and CoCrFeCuMnNi alloy rods are obtained;

[0082] (2) The CoCrFeCuMnNi alloy rod is subjected to an electrode induction melting gas atomization method to obtain a CoCrFeCuMnNi high entropy alloy powder; the melting temperature in the electrode induction melting gas atomization method is maintained between 1650°C and 1680°C, the holding temperature is maintained between 1320°C and 1340°C, and the refining time is 5-10min.

[0083] In the CoCrFeCuMnNi high entropy alloy powder,

[0084]

[0085] The metal ceramic powder is prepared by the following steps:

[0086] Step 1: CoCrFeCuMnNi high entropy alloy powder, SiO 2 The powder and surfactant are put into an appropriate amount of deionized water and stirred for 1-2 hours under ultrasonic conditions to obtain suspension a.

[0087] Step 2: Add urea to suspension a and stir for 10 to 30 minutes to obtain suspension b.

[0088] Step 3: transfer the suspension b to a stainless steel autoclave and perform hydrothermal treatment at 140-180° C. for 2-6 h; then centrifuge at 10,000-15,000 rpm, remove the lower precipitate, and dry at 90-110° C. for 4-6 h to obtain a precursor powder.

[0089] Step 4: heat-treating the precursor powder in an inert gas atmosphere at 1400-1500° C. for 1-3 hours to obtain a metal ceramic powder.

[0090] Example 3

[0091] A metal part surface processing method includes the steps of thermally spraying metal ceramic powder on a stainless steel substrate;

[0092] The metal ceramic powder is composed of the following raw materials by weight:

[0093]

[0094] The CoCrFeCuMnNi high entropy alloy powder is prepared by the following steps:

[0095] 1) Cut Fe, Cu, Co, Ni, Cr and Mn elemental small pieces into pieces no larger than 4 cm 3 Single-substance small pieces, and wash and dry them; when melting the above-mentioned single-substance small pieces, put Cu, Mn, Co, Fe, Ni and Cr element single-substance small pieces into a medium frequency induction furnace in the order of melting point from low to high; the parameters of the medium frequency induction furnace smelting are: slowly increase the induction furnace smelting power at a speed of 3-5kW / 5min, so that the smelting power reaches 35-40kW, and the smelting time is 3-6h, and CoCrFeCuMnNi alloy rods are obtained;

[0096] (2) The CoCrFeCuMnNi alloy rod is subjected to an electrode induction melting gas atomization method to obtain a CoCrFeCuMnNi high entropy alloy powder; the melting temperature in the electrode induction melting gas atomization method is maintained between 1650°C and 1680°C, the holding temperature is maintained between 1320°C and 1340°C, and the refining time is 5-10min.

[0097] In the CoCrFeCuMnNi high entropy alloy powder,

[0098]

[0099] The metal ceramic powder is prepared by the following steps:

[0100] Step 1: CoCrFeCuMnNi high entropy alloy powder, SiO 2 The powder and surfactant are put into an appropriate amount of deionized water and stirred for 1-2 hours under ultrasonic conditions to obtain suspension a.

[0101] Step 2: Add urea to suspension a and stir for 10 to 30 minutes to obtain suspension b.

[0102] Step 3: transfer the suspension b to a stainless steel autoclave and perform hydrothermal treatment at 140-180° C. for 2-6 h; then centrifuge at 10,000-15,000 rpm, remove the lower precipitate, and dry at 90-110° C. for 4-6 h to obtain a precursor powder.

[0103] Step 4: heat-treating the precursor powder in an inert gas atmosphere at 1400-1500° C. for 1-3 hours to obtain a metal ceramic powder.

[0104] Comparative Example 1

[0105] In this comparative example, CoCrFeMnNi high entropy alloy powder is used to replace CoCrFeCuMnNi high entropy alloy powder, and the rest is the same as in Example 2.

[0106] A metal part surface processing method includes the steps of thermally spraying metal ceramic powder on a stainless steel substrate;

[0107] The metal ceramic powder is composed of the following raw materials by weight:

[0108]

[0109] The CoCrFeMnNi high entropy alloy powder is prepared by the following steps:

[0110] 1) Cut Fe, Co, Ni, Cr and Mn elemental small pieces into pieces no larger than 4 cm 3 Single-substance small pieces, and wash and dry them; when melting the above-mentioned single-substance small pieces, put the single-substance small pieces of Mn, Co, Fe, Ni and Cr elements into the medium frequency induction furnace in the order of melting point from low to high; the parameters of the medium frequency induction furnace smelting are: slowly increase the induction furnace smelting power at a speed of 3-5kW / 5min, so that the smelting power reaches 35-40kW, and the smelting time is 3-6h to obtain CoCrFeMnNi alloy rods;

[0111] (2) The CoCrFeMnNi alloy rod is subjected to an electrode induction melting gas atomization method to obtain a CoCrFeMnNi high entropy alloy powder; the melting temperature in the electrode induction melting gas atomization method is maintained between 1650° C. and 1680° C., the holding temperature is maintained between 1320° C. and 1340° C., and the refining time is 5-10 min.

[0112] In the CoCrFeCuMnNi high entropy alloy powder,

[0113]

[0114] The metal ceramic powder is prepared by the following steps:

[0115] Step 1: CoCrFeMnNi high entropy alloy powder, SiO 2 The powder and surfactant are put into an appropriate amount of deionized water and stirred for 1-2 hours under ultrasonic conditions to obtain suspension a.

[0116] Step 2: Add urea to suspension a and stir for 10 to 30 minutes to obtain suspension b.

[0117] Step 3: transfer the suspension b to a stainless steel autoclave and perform hydrothermal treatment at 140-180° C. for 2-6 h; then centrifuge at 10,000-15,000 rpm, remove the lower precipitate, and dry at 90-110° C. for 4-6 h to obtain a precursor powder.

[0118] Step 4: heat-treating the precursor powder in an inert gas atmosphere at 1400-1500° C. for 1-3 hours to obtain a metal ceramic powder.

[0119] Comparative Example 2

[0120] This comparative example does not contain SiO 2 Powder, the rest is the same as in Example 2

[0121] A metal part surface processing method includes the steps of thermally spraying metal ceramic powder on a stainless steel substrate;

[0122] The metal ceramic powder is composed of the following raw materials by weight:

[0123]

[0124] The CoCrFeCuMnNi high entropy alloy powder is prepared by the following steps:

[0125] 1) Cut Fe, Cu, Co, Ni, Cr and Mn elemental small pieces into pieces no larger than 4 cm 3 Single-substance small pieces, and wash and dry them; when melting the above-mentioned single-substance small pieces, put Cu, Mn, Co, Fe, Ni and Cr element single-substance small pieces into a medium frequency induction furnace in the order of melting point from low to high; the parameters of the medium frequency induction furnace smelting are: slowly increase the induction furnace smelting power at a speed of 3-5kW / 5min, so that the smelting power reaches 35-40kW, and the smelting time is 3-6h, and CoCrFeCuMnNi alloy rods are obtained;

[0126] (2) The CoCrFeCuMnNi alloy rod is subjected to an electrode induction melting gas atomization method to obtain a CoCrFeCuMnNi high entropy alloy powder; the melting temperature in the electrode induction melting gas atomization method is maintained between 1650°C and 1680°C, the holding temperature is maintained between 1320°C and 1340°C, and the refining time is 5-10min.

[0127] In the CoCrFeCuMnNi high entropy alloy powder,

[0128]

[0129]

[0130] The metal ceramic powder is prepared by the following steps:

[0131] Step 1: CoCrFeCuMnNi high entropy alloy powder, SiO 2 The powder and surfactant are put into an appropriate amount of deionized water and stirred for 1-2 hours under ultrasonic conditions to obtain suspension a.

[0132] Step 2: Add urea to suspension a and stir for 10 to 30 minutes to obtain suspension b.

[0133] Step 3: transfer the suspension b to a stainless steel autoclave and perform hydrothermal treatment at 140-180° C. for 2-6 h; then centrifuge at 10,000-15,000 rpm, remove the lower precipitate, and dry at 90-110° C. for 4-6 h to obtain a precursor powder.

[0134] Step 4: heat-treating the precursor powder in an inert gas atmosphere at 1400-1500° C. for 1-3 hours to obtain a metal ceramic powder.

[0135] Comparative Example 3

[0136] This comparative example does not contain SiO 2 Powder, replacing the CoCrFeCuMnNi high entropy alloy powder with CoCrFeMnNi high entropy alloy powder, and the rest is the same as Example 2.

[0137] A metal part surface processing method includes the steps of thermally spraying metal ceramic powder on a stainless steel substrate;

[0138] The metal ceramic powder is composed of the following raw materials by weight:

[0139] CoCrFeMnNi high entropy alloy powder 100 parts

[0140] 15 parts surfactant

[0141] 8 parts of urea.

[0142] The CoCrFeMnNi high entropy alloy powder is prepared by the following steps:

[0143] 1) Cut Fe, Co, Ni, Cr and Mn elemental small pieces into pieces no larger than 4 cm 3Single-substance small pieces, and wash and dry them; when melting the above-mentioned single-substance small pieces, put the single-substance small pieces of Mn, Co, Fe, Ni and Cr elements into the medium frequency induction furnace in the order of melting point from low to high; the parameters of the medium frequency induction furnace smelting are: slowly increase the induction furnace smelting power at a speed of 3-5kW / 5min, so that the smelting power reaches 35-40kW, and the smelting time is 3-6h to obtain CoCrFeMnNi alloy rods;

[0144] (2) The CoCrFeMnNi alloy rod is subjected to an electrode induction melting gas atomization method to obtain a CoCrFeMnNi high entropy alloy powder; the melting temperature in the electrode induction melting gas atomization method is maintained between 1650° C. and 1680° C., the holding temperature is maintained between 1320° C. and 1340° C., and the refining time is 5-10 min.

[0145] In the CoCrFeMnNi high entropy alloy powder,

[0146]

[0147] The metal ceramic powder is prepared by the following steps:

[0148] Step 1: Place CoCrFeMnNi high entropy alloy powder and surfactant into an appropriate amount of deionized water, and stir for 1-2 hours under ultrasonic conditions to obtain a suspension a.

[0149] Step 2: Add urea to suspension a and stir for 10 to 30 minutes to obtain suspension b.

[0150] Step 3: transfer the suspension b to a stainless steel autoclave and perform hydrothermal treatment at 140-180° C. for 2-6 h; then centrifuge at 10,000-15,000 rpm, remove the lower precipitate, and dry at 90-110° C. for 4-6 h to obtain a precursor powder.

[0151] Step 4: heat-treating the precursor powder in an inert gas atmosphere at 1400-1500° C. for 1-3 hours to obtain a metal ceramic powder.

[0152] Test Example 1

[0153] The metal ceramic powders of Examples 1-3 and Comparative Examples 1-3 were thermally sprayed on the surface of a stainless steel substrate, with a spraying thickness of 100 μm.

[0154] Follow the spraying method below:

[0155] (1) Surface pretreatment: Pretreat the surface of the stainless steel substrate to remove surface burrs and rust, so that the rust removal level of the stainless steel substrate surface is not less than Sa3.0;

[0156] (2) Thermal spraying: placing the metal ceramic powder into a thermal spraying system, and thermally spraying the metal powder onto the surface of the stainless steel substrate to form a coating.

[0157] The step (2) of thermal spraying using a metal powder spraying torch comprises the following steps:

[0158] (21) Use an oxyacetylene flame to heat the surface of the stainless steel substrate to about 400-500°C, then keep the nozzle 120-150mm away from the surface of the stainless steel substrate, spray the metal ceramic powder evenly on the surface of the workpiece, and then melt it with the flame until the surface has a mirror reflection, and then gradually move the melting position to make the alloy powder and the stainless steel substrate melt and diffuse with each other to form a strong bonding layer.

[0159] The above method uses the following Figure 1 Processing equipment: including a workbench 100, a metal powder spraying welding torch 200, a lifting mechanism 300, a base 400, a power supply mechanism 500 and a walking mechanism 600; the workbench 100 is a rectangular plane workbench, a storage rack 110 is arranged on the other side of the workbench 100, and a clamping device 120 is arranged on the periphery of the storage rack 110; the workbench 100 is installed as a whole on the base 400; the metal powder spraying welding torch 200 is arranged on one side of the workbench 100, and a lifting mechanism 300 is installed below the metal powder spraying welding torch 200; the lifting mechanism 300 is installed on the base 400; the base 400 is hollow, in which a power supply mechanism 500 is arranged; a walking mechanism is arranged below the base 400.

[0160] In order to demonstrate the use of CoCrFeCuMnNi high entropy alloy powder and the addition of SiO 2 In order to demonstrate the beneficial effects of the powder, the metal anti-corrosion coating prepared as above was subjected to the following tests.

[0161] Test 1

[0162] The anti-corrosion experiments on metal anti-corrosion coatings are carried out using conventional neutral salt spray tests and acid immersion tests.

[0163] The results are shown in Table 1 and Figure 2 and Figure 3

[0164] Table 1 Coating anticorrosion performance test.

[0165]

[0166] From the comparison between Comparative Example 1 and Comparative Example 3 in the data of Table 1 above and Example 2, it can be seen that using CoCrFeCuMnNi high entropy alloy powder instead of CoCrFeMnNi high entropy alloy powder can greatly improve the corrosion resistance of the metal coating.

[0167] Test 2

[0168] The mechanical properties of the metal coating were tested, including wear resistance and impact resistance. The results are shown in Table 2 and Figure 4-5 shown.

[0169]

[0170]

[0171] From the comparison of Examples 1-3 and Comparative Examples 1-3 in Table 2, it can be seen that the addition of SiO 2 The powder can significantly reduce its friction coefficient at high temperatures, has certain high-temperature friction-resistant adaptive characteristics, gives it good wear resistance, and adds SiO 2 Powder and CoCrFeCuMnNi high entropy alloy powder can greatly improve its impact resistance.

[0172] From the above embodiments, it can be seen that:

[0173] The invention discloses a metal part surface processing method and a processing device thereof. The invention improves the existing CoCrFeMnNi high entropy alloy powder, adds a specific content of Cu component therein, forms CoCrFeCuMnNi high entropy alloy powder, and further adds SiO 2 The powder is made into a metal ceramic powder. It is found that when the metal ceramic powder is used for thermal spraying, it is better than the CoCrFeMnNi high entropy alloy powder without adding Cu component and the CoCrFeMnNi high entropy alloy powder without adding SiO 2 The corrosion resistance and wear resistance of the powder are greatly increased, which can significantly extend the service life of metal parts. It is particularly suitable for application scenarios with high requirements for wear resistance and corrosion resistance. At the same time, the present invention also discloses equipment that can conveniently use the above method to process the surface of metal parts.

[0174] The above are limited to several preferred embodiments of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A metal surface processing method, It is characterized in that The method comprises the steps of thermally spraying a metal ceramic powder onto a stainless steel substrate; The metal ceramic powder is composed of the following raw materials by weight:

2. A metal part surface processing method according to claim 1, It is characterized in that The CoCrFeCuMnNi high entropy alloy powder is prepared by the following steps: 1) Cut Fe, Cu, Co, Ni, Cr and Mn elemental small pieces into pieces no larger than 4 cm 3 Single-substance small pieces, and wash and dry them; when melting the above-mentioned single-substance small pieces, put Cu, Mn, Co, Fe, Ni and Cr element single-substance small pieces into a medium frequency induction furnace in the order of melting point from low to high; the parameters of the medium frequency induction furnace smelting are: slowly increase the induction furnace smelting power at a speed of 3-5kW / 5min, so that the smelting power reaches 35-40kW, and the smelting time is 3-6h, and CoCrFeCuMnNi alloy rods are obtained; (2) The CoCrFeCuMnNi alloy rod is subjected to an electrode induction melting gas atomization method to obtain a CoCrFeCuMnNi high entropy alloy powder; the melting temperature in the electrode induction melting gas atomization method is maintained between 1650°C and 1680°C, the holding temperature is maintained between 1320°C and 1340°C, and the refining time is 5-10min.

3. A metal surface processing method according to claim 2, It is characterized in that Calculated by weight, in the CoCrFeCuMnNi high entropy alloy powder, 4. A metal surface processing method according to claim 1, It is characterized in that The metal ceramic powder is prepared by the following steps: Step 1: CoCrFeCuMnNi high entropy alloy powder, SiO 2 The powder and surfactant are placed in an appropriate amount of deionized water and stirred for 1-2 hours under ultrasonic conditions to obtain a suspension a; Step 2, adding urea to suspension a, stirring for 10 to 30 minutes, to obtain suspension b; Step 3, the suspension b is transferred to a stainless steel autoclave, and hydrothermally treated at 140-180° C. for 2-6 hours; then centrifuged at 10000-15000 rpm, the lower precipitate is removed, and dried at 90-110° C. for 4-6 hours to obtain a precursor powder; Step 4: heat-treating the precursor powder in an inert gas atmosphere at 1400-1500° C. for 1-3 hours to obtain a metal ceramic powder.

5. A metal part surface processing method according to claim 4, It is characterized in that The particle size of the metal ceramic powder is in the range of 1-30 μm.

6. A metal surface processing method according to claim 1, It is characterized in that The processing method comprises the following steps: (1) Surface pretreatment: Pretreat the surface of the stainless steel substrate to remove surface burrs and rust, so that the rust removal level of the stainless steel substrate surface is not less than Sa3.0; (2) Thermal spraying: placing the metal ceramic powder into a thermal spraying system, and thermally spraying the metal powder onto the surface of the stainless steel substrate to form a coating.

7. A metal surface processing method according to claim 1, It is characterized in that The step (2) of thermal spraying using a metal powder spraying torch comprises the following steps: (21) Use an oxyacetylene flame to heat the surface of the stainless steel substrate to about 400-500°C, then keep the nozzle 120-150mm away from the surface of the stainless steel substrate, spray the metal ceramic powder evenly on the surface of the workpiece, and then melt it with the flame until the surface has a mirror reflection, and then gradually move the melting position to make the alloy powder and the stainless steel substrate melt and diffuse with each other to form a strong bonding layer.

8. A processing device, It is characterized in that Used in the metal part surface processing method described in any one of claims 1-6.

9. A processing device according to claim 8, It is characterized in that The invention comprises a workbench (100), a metal powder spraying welding torch (200), a lifting mechanism (300), a base (400), a power supply mechanism (500) and a walking mechanism (600); the workbench (100) is a rectangular plane workbench, a storage rack (110) is arranged on the other side of the workbench (100), and a clamping device (120) is arranged on the periphery of the storage rack (110); the workbench (100) is integrally mounted on the base (400); the metal powder spraying welding torch (200) is arranged on one side of the workbench (100), and a lifting mechanism (300) is arranged below the metal powder spraying welding torch (200); the lifting mechanism (300) is mounted on the base (400); the base (400) is hollow, and a power supply mechanism (500) is arranged therein; and a walking mechanism is arranged below the base (400).

Citation Information

Patent Citations

  • Supersonic flame spraying equipment and coating method thereof

    CN109943798A

  • Preparation method of MnCoCrFeNi high-entropy alloy nanocrystalline coating

    CN111945098A

  • (CoCrFeMnNi) N high-entropy ceramic powder and preparation method thereof

    CN114804887A

  • High-strength and ultra heat-resistant high entropy alloy (HEA) matrix composites and method of preparing the same

    US20170314097A1

Cited By

  • Plasma thermal spraying-hot rolling in-situ forming system and method for titanium alloy ultrahigh-temperature ceramic coating

    CN119640196A