Self-adaptive infrared stealth flexible film compatible with visible light camouflage
By introducing doped VO2 layer and metal nanolayer into infrared stealth materials, combined with the transmissive layer, the adjustment of infrared emissivity and visible light transmittance is achieved, and the problem of single band and insufficient compatibility of infrared stealth materials is solved, and the self-reliance is achieved Adapt to the compatibility of infrared stealth and visible light camouflage, improving the multi-band stealth effect.
Patent Information
- Application Number
- CN202410974652.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-15
AI Technical Summary
The existing infrared stealth materials have a single band and are not compatible with visible light camouflage camouflage, and cannot effectively disguise the target in a multi-band environment. The diversified detection methods lead to insufficient single-band stealth materials.
Provide an adaptive infrared stealth flexible film compatible with visible light camouflage, including doped VO2 layer, metal nanolayer and impermeable layer. Through the coating step and material combination, it can achieve variable infrared emissivity and high visible light transmission and regulate infrared radiation. Characteristics to adapt to environmental changes.
The compatibility between infrared stealth and visible light camouflage is achieved. The visible light transmittance of the film exceeds 75%, the phase transition temperature is adjustable, and the surface infrared emissivity decreases with the increase of temperature, achieving an adaptive infrared stealth effect.
Smart Images

Figure CN118957488A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of functional films, and in particular relates to an adaptive infrared stealth flexible film compatible with visible light camouflage. Background Art
[0002] All objects with a temperature above absolute zero have infrared radiation. According to the Stefan-Boltzmann law [8]: E = εδT4 (where E is the total radiation intensity, W / m2; ε is the total emissivity of the object; δ is the Boltzmann constant, W / (m2·K4); and T is the absolute temperature of the target, K), the infrared radiation energy of an object mainly depends on the surface temperature of the object and its infrared emissivity. Based on the ubiquity of infrared radiation, by effectively controlling or managing the infrared radiation characteristics of the target and reducing or eliminating the infrared radiation difference between the target and the background, the detectability of the target in the infrared band can be reduced, infrared stealth technology can be realized, and the initiative on the battlefield can be mastered. In order to achieve infrared stealth, it is necessary to try to reduce the thermal radiation difference between the target and the background. The most effective ways include: first, controlling the surface temperature of the target so that the temperature difference between the detected target and the surrounding environment is as small as possible, which can be achieved through insulation, heat dissipation, or phase change absorption of phase change materials; second, adjusting the emissivity of the target surface so that the infrared radiation difference between the target and the background is as small as possible.
[0003] In recent years, the research and application of infrared stealth materials such as low infrared emissivity coatings have been extensive, with the goal of changing the emissivity of the target surface by adjusting the emissivity of the target surface. However, since the infrared radiation characteristics of the target background change with the background topography, time, temperature, etc., when the background changes during movement, it is not possible to effectively camouflage the target by simply using low emissivity materials; on the other hand, with the diversification of detection methods, the detection process may use visible light / infrared compatible detection methods, and single-band stealth materials cannot meet actual application needs.
[0004] In order to improve the development efficiency of multi-band stealth materials and reduce costs, it is necessary to be compatible with the existing visible light camouflage layer. The stealth mechanisms of existing infrared stealth materials and visible light camouflage layers are different, and the material performance requirements of the two will restrict each other to a certain extent. Therefore, in order to make the infrared stealth layer have the characteristics of adaptability and compatibility with the existing visible light camouflage, it is necessary to study infrared emissivity variable materials with high visible light transmittance. Summary of the invention
[0005] The purpose of the present invention is to provide a variable infrared emissivity material with high visible light transmittance to address the problem that the infrared stealth materials in the prior art have a single wavelength band and are not compatible with visible light camouflage.
[0006] In order to achieve the above object, the present invention provides the following technical solution, providing an adaptive infrared stealth flexible film compatible with visible light camouflage, the film comprising: a substrate, a doped VO2 layer, a metal nanolayer and an anti-reflection layer arranged in sequence,
[0007] Wherein, the doped VO2 layer is a doped VO2 thin film doped with metal oxide.
[0008] The adaptive infrared stealth flexible film compatible with visible light camouflage provided in the present application also has the following characteristics: the coating steps of the doped VO2 film are as follows:
[0009] S1: Clean the substrate by ultrasonic cleaning in acetone for 15 min and ultrasonic cleaning in analytical grade isopropanol for 15 min;
[0010] S2: Place the sample in the magnetron sputtering coating machine, move the baffle between the sample and the target, and evacuate the sample;
[0011] S3: introduce protective gas;
[0012] S4: Sputtering target cleaning, sputtering power 100W-200W, sputtering time not less than 15min;
[0013] S5: substrate bias cleaning;
[0014] S6: Remove the baffle between the sample and the target and perform sputtering deposition. The sputtering power is controlled at 100W to 200W and the deposition time is 20 to 60 minutes.
[0015] The adaptive infrared stealth flexible film compatible with visible light camouflage provided in the present application also has the following characteristics: the target material is a mixed target material of VO2 and WO3, wherein the mass fraction of WO3 is 2% to 50%, the target material thickness is 3 mm, and the diameter is 76.2 mm.
[0016] The adaptive infrared stealth flexible film compatible with visible light camouflage provided in the present application also has the following characteristics: the target material is a mixed target material of VO2 and MoO3, wherein the mass fraction of MoO3 is 2% to 50%, the target material thickness is 3 mm, and the diameter is 76.2 mm.
[0017] The adaptive infrared stealth flexible film compatible with visible light camouflage provided in the present application also has the following characteristics: the metal nanolayer includes a metal nanowire mixed solution, the metal nanowire mixed solution includes metal nanowires, the metal nanowires have a diameter of 20 to 60 nm, a length of 2 to 30 μm, and a concentration in the dispersion of 2 to 80 mg / mL.
[0018] The adaptive infrared stealth flexible film compatible with visible light camouflage provided in the present application also has the following characteristics: the metal nanowire mixed solution includes, by mass percentage:
[0019] Metal nanowires 1-5%
[0020] Dimethyl sulfoxide 1-7%
[0021] Acrylic resin 2-5%
[0022] Polyurethane resin 0.2-2%
[0023] Leveling agent 0.1-0.2%
[0024] Wetting agent 0.1-0.2%
[0025] Solvent 80.6%-95.6%,
[0026] Wherein, the solvent is a deionized water solution of isopropanol.
[0027] The adaptive infrared stealth flexible film compatible with visible light camouflage provided in the present application also has the following characteristics: the metal nanowire mixed solution is coated on a substrate by a method selected from spin coating, immersion pulling, scraping and spraying, and the substrate is a substrate plated with a doped VO2 film.
[0028] The adaptive infrared stealth flexible film compatible with visible light camouflage provided in the present application also has the following characteristics: the spin coating method comprises the following steps:
[0029] A. Before using the substrate, soak it in acetone and ultrasonically clean it for 20 minutes;
[0030] B. Soak in isopropanol, ultrasonically clean for 20 minutes, and blow dry with nitrogen;
[0031] C. Place the cleaned substrate in the center of the rotating platform of the spin coater, turn on the suction pump, and set the spin coating time and speed;
[0032] D. Drop the mixed solution in the center of the substrate, then turn on the spin coater and start spin coating;
[0033] E. When the rotation stops, turn off the suction pump, remove the sample, and place it in a vacuum oven at 30°C. Keep the vacuum for at least 1 hour.
[0034] The adaptive infrared stealth flexible film compatible with visible light camouflage provided in the present application also has the following characteristics: the immersion and pulling method adopts an immersion and pulling coating machine for coating, with a descending speed of 1 to 5 mm / s, a pulling rising speed of 1 to 5 mm / s, an immersion time of 20 to 50 s, a stop time of 60 s, and 2 to 50 coating times.
[0035] The adaptive infrared stealth flexible film compatible with visible light camouflage provided in the present application also has the following characteristics: the periphery of the anti-reflection layer also includes a protective layer, and the protective layer includes 2% acrylate, 1% polyurethane, 0.2% active diluent, 0.05% coupling agent, 1% ultraviolet absorber, 10% conductive polymer and 85.75% protective layer solvent.
[0036] Beneficial Effects
[0037] The adaptive infrared stealth flexible film compatible with visible light camouflage provided by the present invention has a visible light transmittance of more than 75%; through doping, the phase transition temperature can be continuously adjusted from room temperature to 68°C, and the surface infrared emissivity decreases from 0.85 to 0.5 as the temperature increases. The color of the film is usually dark green, dark brown or blue-brown at room temperature, and can be used as a camouflage patch. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0039] Figure 1 A schematic diagram of the structure of an adaptive infrared stealth flexible film compatible with visible light camouflage provided by an embodiment of the present invention;
[0040] Figure 2 The infrared thermal image of the adaptive infrared stealth flexible film compatible with visible light camouflage provided by the embodiment of the present invention,
[0041] Figure 3 Provided for Example 1 are optical camouflage photos of an adaptive infrared stealth flexible film compatible with visible light camouflage and its corresponding infrared imaging at 30°C,
[0042] Figure 4 The optical camouflage photo of the adaptive infrared stealth flexible film compatible with visible light camouflage provided in Example 2 and its corresponding infrared imaging at 40°C. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below in conjunction with examples, but it should be noted that these implementation modes are not limitations of the present invention, and any equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in the field based on these implementation modes are all within the protection scope of the present invention.
[0044] The embodiment of the present invention provides an adaptive infrared stealth flexible film compatible with visible light camouflage, such as Figure 1 As shown, the film includes: a substrate, a doped VO2 layer, a metal nanolayer, an anti-reflection layer and a protective layer arranged in sequence, wherein the doped VO2 layer is a doped VO2 film doped with metal oxide. The unique metal-semiconductor transition (MIT) characteristic of VO2-based films is utilized, that is, as the temperature increases, the crystal structure undergoes a phase change, from a semiconductor state to a metallic state. When vanadium oxides undergo a phase change, their optical properties in the visible light region do not change much, but their optical characteristics in the infrared band undergo a significant change, that is, as the temperature increases, the infrared band changes from high transmittance to high reflectivity. Utilizing this characteristic of the material, the transmittance and reflectivity of infrared radiation can be automatically adjusted with changes in ambient temperature, that is, as the temperature increases, the emissivity decreases synchronously, thereby achieving the purpose of adaptive infrared stealth. Since higher temperatures will greatly increase infrared radiation, it is necessary to lower the phase change temperature of the film. The phase change temperature of pure VO2 is 68°C, which is much higher than the ambient temperature. By doping and other methods, its phase change temperature can be changed, and high-valent ions (such as Nb 5+ , 5+ , W 6+ etc.) can lower its temperature, and doping with low-valent ions (such as Al 3+ Cr 3+ , Fe 3+ The phase transition temperature can be increased by adjusting the phase transition temperature according to actual needs. The thickness of the doped VO2 film, the type of doped metal oxide and the doping content can be selected according to actual needs to achieve different effects.
[0045] In the above embodiment, highly transparent PET is selected as the substrate, and a flexible film can be directly formed. Different substrates can be selected for functional films. If the existing camouflage cloth needs to have the performance of adaptive infrared stealth compatible with visible light camouflage, the camouflage cloth with optical camouflage is used as the substrate, and the coating method or spraying method is used; if the existing camouflage equipment has the performance of adaptive infrared stealth compatible with visible light camouflage, the surface of the equipment with optical camouflage is used as the substrate, and the spraying method is used.
[0046] In some embodiments, the steps of coating the doped VO2 thin film are as follows:
[0047] S1: Clean the substrate by ultrasonic cleaning in acetone for 15 min and ultrasonic cleaning in analytical grade isopropanol for 15 min;
[0048] S2: Place the sample in the magnetron sputtering coating machine, move the baffle between the sample and the target, and evacuate the sample;
[0049] S3: introduce protective gas, the protective gas is argon, the purity is 99.99%, 0.5-1Pa;
[0050] S4: Sputtering target cleaning, sputtering power 100W-200W, sputtering time not less than 15min;
[0051] S5: substrate bias cleaning, voltage 300V-800V, current 0.05A, duty cycle 75%, time 5-15min;
[0052] S6: Remove the baffle between the sample and the target and perform sputtering deposition. The sputtering power is controlled at 100W to 200W and the deposition time is 20 to 60 minutes.
[0053] In the above embodiment, the sputtering process uses Ar with a purity of 99.99%, 0.5 Pa, and the substrate temperature is 300°C.
[0054] In some embodiments, the target material is a mixed target material of VO2 and WO3, wherein the mass fraction of WO3 is 2% to 50%, and the target material has a thickness of 3 mm and a diameter of 76.2 mm.
[0055] In some embodiments, the target material is a mixed target material of VO2 and MoO3, wherein the mass fraction of MoO3 is 2%-50%, and the target material has a thickness of 3 mm and a diameter of 76.2 mm.
[0056] In some embodiments, the metal nanolayer includes a metal nanowire mixed solution, the metal nanowire mixed solution includes metal nanowires, the metal nanowires have a diameter of 20 to 60 nm, a length of 2 to 30 μm, and a concentration of 2 to 80 mg / mL in the dispersion.
[0057] In some embodiments, a metal micro-nano structure layer is added to the phase change layer, and the plasmon anti-reflection effect of the metal micro-nano grid is used to achieve a strong reflection characteristic similar to that of a continuous metal film in the infrared "atmospheric window" band, that is, a low infrared emissivity characteristic. At the same time, a high transmittance characteristic is achieved in the short wave (optical band), that is, the regulation of the multi-band spectrum is achieved. First, a metal micro-nano grid layer is constructed on the surface of the substrate using metal nanowires. The types of metal nanowires selected are Ag, Ni, Cu, and Au nanowires, but are not limited thereto.
[0058] In some embodiments, the metal nanowire mixed solution includes, by mass percentage:
[0059] Metal nanowires 1-5%
[0060] Dimethyl sulfoxide 1-7%
[0061] Acrylic resin 2-5%
[0062] Polyurethane resin 0.2-2%
[0063] Leveling agent 0.1-0.2%
[0064] Wetting agent 0.1-0.2%
[0065] Solvent 80.6%-95.6%,
[0066] Wherein, the solvent is a deionized water solution of isopropanol.
[0067] In some embodiments, the metal nanowire mixed solution is coated on a substrate by a method selected from spin coating, dip coating, doctor blade coating and spray coating, and the substrate is a substrate coated with a doped VO2 thin film.
[0068] In some embodiments, the spin coating method uses a spin coater to perform spin coating, and the steps of the spin coating method are as follows:
[0069] A. Before using the substrate, soak it in acetone and ultrasonically clean it for 20 minutes;
[0070] B. Soak in isopropanol, ultrasonically clean for 20 minutes, and blow dry with nitrogen;
[0071] C. Place the cleaned substrate in the center of the rotating platform of the spin coater, turn on the suction pump, and set the spin coating time and speed; the suction pump is used to ensure that the glass does not fly out during rotation, the acceleration time is 10 seconds, the uniform speed time is 50 seconds, and the total is 60 seconds; the speed is 400-2000rpm;
[0072] D. Drop the mixed solution in the center of the substrate, then turn on the spin coater and start spin coating;
[0073] E. When the rotation stops, turn off the suction pump, remove the sample, and place it in a vacuum oven at 30°C for at least 1 hour. Keeping it for one hour ensures that the solvent in the film evaporates to form a uniform nano-metamaterial film.
[0074] In some embodiments, the parameters of the spraying method are: nozzle diameter 0.1-2 mm, spray gun distance 15-30 cm, spraying air pressure 2.0 bar, spray gun moving speed 1-10 mm / s.
[0075] In some embodiments, the parameters of the coating method are: using a scraper, heating the sample stage to 80-100° C., using a 1-10 μm wire bar scraper, and coating at a relative speed of 1-10 mm / s with the coating head to the substrate.
[0076] In some embodiments, the dip-coating method uses a dip-coating machine for coating, with a descending speed of 1-5 mm / s, a pulling rising speed of 1-5 mm / s, a dipping time of 20-50 s, a stop time of 60 s, and a coating number of 2-50 times. It also includes vacuum drying the film in a vacuum drying oven, with a drying temperature of 30° C. and a drying time of more than 1 hour.
[0077] In some embodiments, the scraping method is as follows: a scraping machine is used, the sample stage is heated to 80-100° C., and a 1-10 μm wire bar scraper is used to apply the coating at a speed of 1-10 mm / s.
[0078] In some embodiments, the anti-reflection layer includes SiO2.
[0079] In the above embodiment, a SiO2 anti-reflection layer is plated on the surface of the VO2 film to make the rate of change of the refractive index between the film layers become gentle, thereby effectively reducing the reflected energy and further improving the transmittance of visible light. The SiO2 anti-reflection layer is deposited by magnetron sputtering, using a SiO2 target material with a purity of 99.999%, a target material thickness of 3mm and a diameter of 76.2mm. The sputtering process uses Ar with a purity of 99.99% and 0.5Pa, and the SiO2 film is deposited at room temperature. The deposition process is as follows: put the sample into the magnetron sputtering coating machine, move the baffle between the sample and the target, and evacuate; clean the target material by air sputtering; sputter deposition, and the sputtering power is controlled at 100W to 200W. The deposition time is 10 to 30 minutes, and SiO2 films of different thicknesses can be obtained.
[0080] In some embodiments, the protective layer includes 2% acrylate, 1% polyurethane, 0.2% reactive diluent, 0.05% coupling agent, 1% UV absorber, 10% conductive polymer and 85.75% protective layer solvent.
[0081] In the above embodiment, the protective layer is coated on the surface of the film to improve the environmental resistance of the film. A film scraping machine can be used, the sample stage is heated to 100°C, and a 1-5μm wire rod scraper is used to coat at a speed of 1-10mm / s.
[0082] In the above embodiment, Figure 2 The infrared imaging diagrams of the film provided in the above embodiment at different temperatures show that as the temperature increases, the infrared emissivity of the film surface decreases, indicating that the film has an adaptive red stealth effect.
[0083] Embodiment 1
[0084] The base material is a camouflage fabric with a visible light camouflage coating.
[0085] Using the magnetron sputtering method, the target material is VO2 (92at%)-WO3 (8at%), and the coating steps of the doped VO2 film are as follows:
[0086] S1: Clean the substrate by ultrasonic cleaning in acetone for 15 min and ultrasonic cleaning in analytical grade isopropanol for 15 min;
[0087] S2: Place the sample in the magnetron sputtering coating machine, move the baffle between the sample and the target, and evacuate the sample;
[0088] S3: introduce argon gas with a purity of 99.99% and a concentration of 0.5-1 Pa;
[0089] S4: Sputtering target cleaning, sputtering power 100W, sputtering time 15min;
[0090] S5: substrate bias cleaning, voltage 300 V, current 0.05 A, duty cycle 75%, time 15 min;
[0091] S6: The baffle between the sample and the target is removed, and sputtering deposition is performed. The sputtering power is controlled at 200 W and the deposition time is 60 min.
[0092] A VO2 film with a thickness of about 300 nm and a W-doped content of 6 to 8 at% was obtained.
[0093] The metal nanowire mixed solution was sprayed on the doped VO2 film, and the nozzle diameter of the spray gun was selected to be 0.5 mm, the spray gun distance was 15 cm, the spraying pressure was 2.0 bar, and the spray gun moving speed was 5 mm / s.
[0094] Finally, magnetron sputtering is used to deposit a SiO2 film of ~300 nm.
[0095] Optical camouflage photos and their corresponding infrared images at 30°C are shown in Figure 3 , with good infrared stealth characteristics that are compatible with visible light camouflage.
[0096] Embodiment 2
[0097] Choose a highly transparent PET substrate.
[0098] Using the magnetron sputtering method, the target material is VO2 (95at%)-WO3 (5at%), and the coating steps of the doped VO2 film are as follows:
[0099] S1: Clean the substrate by ultrasonic cleaning in acetone for 15 min and ultrasonic cleaning in analytical grade isopropanol for 15 min;
[0100] S2: Place the sample in the magnetron sputtering coating machine, move the baffle between the sample and the target, and evacuate the sample;
[0101] S3: introduce argon gas with a purity of 99.99% and a concentration of 0.5-1 Pa;
[0102] S4: Sputtering target cleaning, sputtering power 100W, sputtering time 15min;
[0103] S5: substrate bias cleaning, voltage 300 V, current 0.05 A, duty cycle 75%, time 15 min;
[0104] S6: The baffle between the sample and the target is removed, and sputtering deposition is performed. The sputtering power is controlled at 200 W and the deposition time is 60 min.
[0105] A VO2 film with a thickness of about 300 nm and a W-doped content of 3 to 5 at% is obtained.
[0106] The metal nanowire mixed solution was coated on the doped VO2 film by blade coating. A blade coating machine was used, the sample stage was heated to 80°C, and a 1μm wire rod was used at a speed of 5mm / s.
[0107] Finally, magnetron sputtering is used to deposit a SiO2 film of ~300 nm.
[0108] Optical camouflage photos and their corresponding infrared images at 40°C are shown in Figure 4 .
[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.
Claims
1. An adaptive infrared stealth flexible film compatible with visible light camouflage, characterized in that: The film includes: a substrate, a doped VO2 layer, a metal nanolayer and an anti-reflection layer arranged in sequence, Wherein, the doped VO2 layer is a doped VO2 thin film doped with metal oxide.
2. The adaptive infrared stealth flexible film compatible with visible light camouflage according to claim 1, characterized in that: The coating steps of the doped VO2 film are as follows: S1: Clean the substrate by ultrasonic cleaning in acetone for 15 min and ultrasonic cleaning in analytical grade isopropanol for 15 min; S2: Place the sample in the magnetron sputtering coating machine, move the baffle between the sample and the target, and evacuate the sample; S3: introduce protective gas; S4: Sputtering target cleaning, sputtering power 100W-200W, sputtering time not less than 15min; S5: substrate bias cleaning; S6: Remove the baffle between the sample and the target and perform sputtering deposition. The sputtering power is controlled at 100W to 200W and the deposition time is 20 to 60 minutes.
3. The adaptive infrared stealth flexible film compatible with visible light camouflage according to claim 2 is characterized in that: The target material is a mixed target material of VO2 and WO3, wherein the mass fraction of WO3 is 2% to 50%, the target material has a thickness of 3 mm and a diameter of 76.2 mm.
4. The adaptive infrared stealth flexible film compatible with visible light camouflage according to claim 2, characterized in that: The target material is a mixed target material of VO2 and MoO3, wherein the mass fraction of MoO3 is 2%-50%, the target material has a thickness of 3 mm and a diameter of 76.2 mm.
5. The adaptive infrared stealth flexible film compatible with visible light camouflage according to claim 1, characterized in that: The metal nanolayer includes a metal nanowire mixed solution, and the metal nanowire mixed solution includes metal nanowires. The metal nanowires have a diameter of 20 to 60 nm, a length of 2 to 30 μm, and a concentration of 2 to 80 mg / mL in the dispersion.
6. The adaptive infrared stealth flexible film compatible with visible light camouflage according to claim 5, characterized in that: The metal nanowire mixed solution includes, by mass percentage: Metal nanowires 1-5% Dimethyl sulfoxide 1-7% Acrylic resin 2-5% Polyurethane resin 0.2-2% Leveling agent 0.1-0.2% Wetting agent 0.1-0.2% Solvent 80.6%-95.6%, Wherein, the solvent is a deionized water solution of isopropanol.
7. The adaptive infrared stealth flexible film compatible with visible light camouflage according to any one of claims 5 to 6, characterized in that: The metal nanowire mixed solution is coated on a substrate by a method selected from spin coating, dip coating, scraping and spraying, and the substrate is a substrate for plating a doped VO2 film.
8. The adaptive infrared stealth flexible film compatible with visible light camouflage according to claim 7, characterized in that: The spin coating process steps are as follows: A. Before using the substrate, soak it in acetone and ultrasonically clean it for 20 minutes; B. Soak in isopropanol, ultrasonically clean for 20 minutes, and blow dry with nitrogen; C. Place the cleaned substrate in the center of the rotating platform of the spin coater, turn on the suction pump, and set the spin coating time and speed; D. Drop the mixed solution in the center of the substrate, then turn on the spin coater and start spin coating; E. When the rotation stops, turn off the suction pump, remove the sample, and place it in a vacuum oven at 30°C. Keep the vacuum for at least 1 hour.
9. The adaptive infrared stealth flexible film compatible with visible light camouflage according to claim 7, characterized in that: The immersion and pulling method adopts an immersion and pulling coating machine for coating, with a descending speed of 1 to 5 mm / s, a pulling rising speed of 1 to 5 mm / s, an immersion time of 20 to 50 seconds, a stop time of 60 seconds, and 2 to 50 coating times.
10. The adaptive infrared stealth flexible film compatible with visible light camouflage according to claim 1, characterized in that: The anti-transmission layer also includes a protective layer outside, and the protective layer includes 2% acrylate, 1% polyurethane, 0.2% active diluent, 0.05% coupling agent, 1% ultraviolet absorber, 10% conductive polymer and 85.75% protective layer solvent.
Citation Information
Patent Citations
Hypovanadic oxide-based composite film with adjustable radiance and preparation method thereof
CN101817644A
Intelligent temperature-control vanadium dioxide composite multifunctional thin film and preparation method thereof
CN102241482A
Transparent electroconductive film and method for manufacturing same, information input apparatus, and electronic device
CN105960685A
Infrared stealth metal nanoparticle metamaterial composite film compatible with visible light stealth and preparation method thereof
CN110196460A
Anti-reflection anti-repetition composite film for glass substrate and preparation method thereof
CN111830604A
Cited By
Preparation method of flexible conductive film with infrared camouflage effect
CN119724743A
A method for preparing a flexible conductive film with infrared camouflage effect
CN119724743B
Multi-spectrum compatible camouflage and protection film and preparation method thereof
CN121804274A
A multispectral compatible camouflage and protective film and a method for preparing the same
CN121804274B