Copper-based catalyst for coenzyme regeneration as well as preparation method and application of copper-based catalyst
Through the preparation method of copper-based catalyst, the problem of difficulty and low efficiency of separation between catalyst and reaction substrate in coenzyme regeneration is solved, and the regeneration and short regeneration time of high selectivity coenzyme is achieved, which is suitable for large-scale industrial applications.
Patent Information
- Application Number
- CN202411008276.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, it is difficult to separate the coenzyme regeneration catalyst from the reaction substrate, has low efficiency, and precious metal catalysts are not conducive to large-scale industrial applications.
Using the preparation method of copper-based catalyst, the copper substrate is immersed in a functional solution, calcined and electrochemically activated, and a nanowire-shaped copper nanowire catalyst is prepared for electrochemical hydrogenation and regeneration of coenzymes, and the catalyst and reaction are solved. The separation problem of substrates and improves regeneration efficiency.
Regeneration of highly selective coenzymes is achieved, and most of the coenzymes are reduced in a short time, which avoids the difficulty of separation between the catalyst and the reaction substrate, improves the regeneration time and conversion rate, and reduces the generation of by-products.
Smart Images

Figure CN118957629A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of bioelectrochemical catalysis, and specifically relates to a copper-based catalyst for coenzyme regeneration and a preparation method and application thereof. Background Art
[0002] Oxidoreductases catalyze many redox reactions during metabolism and play a key role in bioenergy conduction. Due to their extremely high chemical selectivity, mild reaction conditions and ideal catalytic efficiency, oxidoreductases have great application prospects in the field of organic synthesis. Most of all oxidoreductases require nicotinamide adenine dinucleotide (NADH) as a coenzyme, which refers to the biologically active 1,4-NADH. When using oxidoreductases for biocatalysis, a certain amount of coenzyme will be consumed while synthesizing the product, which will be oxidized to form NAD + , the efficient supply of coenzymes is one of the important technologies for developing redox enzyme catalytic reactions. Adding a large amount of coenzymes is not feasible, and the efficient regeneration of coenzymes becomes the key to biocatalytic reactions.
[0003] Coenzyme regeneration is to regenerate the coenzyme from an oxidized state to a reduced state. Regeneration methods generally include enzymatic method, chemical method, photocatalytic method and electrochemical method. At present, electrochemical coenzyme regeneration mainly adopts rhodium molecular catalyst, which is expensive. When the coenzyme is regenerated, it forms a homogeneous system with the reaction substrate, and it is difficult to separate the rhodium molecular catalyst from the reaction substrate. The prior art also discloses a supported bimetallic nanocatalyst, which is composed of bimetallic nanoparticles supported on a carrier. The bimetallic nanocatalyst is essentially a heterogeneous chemical reduction method, and there is still a problem of difficulty in separating the product and the catalyst, and the complexity of the system is increased. The coenzyme regeneration time is still relatively long, up to several hours, and the catalyst is mainly based on precious metals such as gold and palladium, which is not conducive to large-scale industrial application. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the prior art that the catalyst used for coenzyme regeneration is difficult to separate from the reaction substrate, and the prior art has low coenzyme reduction efficiency, thereby providing a copper-based catalyst for coenzyme regeneration and its preparation method and application.
[0005] To solve the above problems, the present invention provides the following technical solutions.
[0006] The first aspect of the present invention provides a method for preparing a copper-based catalyst for coenzyme regeneration, comprising the following steps:
[0007] (1) immersing a copper substrate in a functional solution to obtain a substrate containing nanowires; wherein the functional solution comprises an alkaline compound and an oxidant;
[0008] (2) calcining and electrochemically activating the nanowire-containing substrate to obtain a copper nanowire catalyst.
[0009] The height of the copper nanowire catalyst is 5 to 10 μm; and / or the diameter of the copper nanowire catalyst is 100 to 300 nm.
[0010] The potential of the electrochemical activation is -1.2 to -0.7 V. The potential is relative to the silver / silver chloride reference electrode. The electrochemical activation is performed by scanning 60 cycles at the potential with a scanning rate of 50 mV / s.
[0011] The calcination temperature is 200-900° C. and the calcination time is 1-3 hours.
[0012] The calcination includes three situations, namely:
[0013] (1) The calcination atmosphere is a nitrogen-containing atmosphere, the calcination temperature is 200 to 400° C., and the calcination time is 1 to 3 hours; or,
[0014] (2) the calcination atmosphere is nitrogen or argon, the calcination temperature is 550-900° C., and the calcination time is 1-3 hours; or,
[0015] (3) The calcination atmosphere is a hydrogen-containing atmosphere, the calcination temperature is 300 to 500° C., and the calcination time is 1 to 3 hours.
[0016] When the calcination satisfies the first condition, the substrate containing copper oxide nanowires is obtained after calcination in step (2); when the calcination satisfies the second condition, the substrate containing cuprous oxide nanowires is obtained after calcination in step (2); when the calcination satisfies the third condition, the substrate containing copper nanowires is obtained after calcination in step (2), and copper oxide exists on the surface of the copper nanowires. Regardless of which condition the calcination satisfies, copper nanowire catalysts are obtained after electrochemical activation. The nitrogen-containing atmosphere can be air, nitrogen, etc. The hydrogen-containing atmosphere is argon containing 5 vol% hydrogen.
[0017] The alkaline compound is at least one of potassium hydroxide and sodium hydroxide;
[0018] Preferably, the oxidant is (NH4)2S2O8;
[0019] Preferably, the concentration of the alkaline compound in the functional solution is 1.3-2.6 mol / L, and the concentration of the oxidant is 0.0325-0.26 mol / L;
[0020] Preferably, the molar ratio of the basic compound to the oxidant is 20:1.
[0021] In the present invention, the copper substrate is pure copper, and the size of the substrate can be selected according to actual conditions, such as a size of 1×1 cm 2 .
[0022] The second aspect of the present invention provides a copper-based catalyst prepared by the above preparation method.
[0023] The third aspect of the present invention provides a method for regenerating a coenzyme, using the copper-based catalyst prepared by the above preparation method.
[0024] The copper-based catalyst is used to electrochemically hydrogenate the coenzyme;
[0025] Preferably, the voltage of the electrochemical reduction is -1.2 to -0.7 V;
[0026] Preferably, the electrochemical reduction time is 20 to 30 minutes.
[0027] The coenzyme is NAD + and NADP + At least one of .
[0028] When electrochemical hydrogenation is carried out, it is carried out at room temperature.
[0029] The coenzyme is NAD + and NADP + At least one of the following: NAD + or NADP + The concentration can be but not limited to 0.5-10 mmol / L.
[0030] The technical solution of the present invention has the following advantages:
[0031] 1. The present invention provides a method for preparing a copper-based catalyst for coenzyme regeneration, the preparation method comprising: (1) immersing a copper substrate in a functional solution to obtain a substrate containing nanowires; wherein the functional solution comprises an alkaline compound and an oxidant; (2) calcining and electrochemically activating the substrate containing nanowires to obtain a copper nanowire catalyst. The copper-based catalyst prepared by the method is in the form of nanowires, which can achieve highly selective coenzyme regeneration and convert NAD +It is reduced to NADH, especially 1,4-NADH with high activity, and overcomes the problem of separation of catalyst and reaction substrate that is difficult to solve in the prior art using homogeneous catalysts. When the copper-based catalyst of the present invention is used for coenzyme regeneration, most of the coenzymes can be reduced in a short time. The present invention uses a copper substrate as a raw material to generate nanowire-shaped Cu(OH)2 under alkaline conditions, and obtains a nanowire-shaped intermediate product after calcination. After activation, a copper nanowire catalyst is obtained. The catalyst is used as a cathode when used, and there is no problem of difficulty in separating the catalyst from the reaction substrate. It can also achieve highly selective coenzyme regeneration with a short regeneration time.
[0032] 2. The method for regenerating coenzymes provided by the present invention, controlling the potential and coenzyme concentration of electrochemical hydrogenation helps to improve the conversion rate, voltage or NAD in the coenzyme + Too high a concentration will result in an increase in by-products. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 In the experimental example of the present invention, the copper nanowire catalyst and the copper substrate of Example 1 are used for the coenzyme NAD + Regeneration, NAD at different regeneration times + concentration;
[0035] Figure 2 In the experimental example of the present invention, the copper nanowire catalyst and the copper substrate of Example 1 are used for the coenzyme NAD + regeneration, 1,4-NADH obtained at different regeneration times;
[0036] Figure 3 In the experimental example of the present invention, the copper nanowire catalyst and the copper substrate of Example 1 are used for the coenzyme NAD + Regeneration, 1,6-NADH obtained at different regeneration times;
[0037] Figure 4 The different initial concentrations of coenzyme NAD in the test examples of the present invention + Regeneration under the action of the copper nanowire catalyst in Example 1;
[0038] Figure 5 The different initial concentrations of coenzyme NAD in the test examples of the present invention + Regeneration under the action of copper substrate;
[0039] Figure 6 In the test examples of the present invention, different initial concentrations of coenzyme NAD + Selectivity under the copper nanowire catalyst and copper substrate in Example 1;
[0040] Figure 7 This is the regeneration of the coenzyme by the copper nanowire catalyst of Example 1 at different voltages in the test examples of the present invention;
[0041] Figure 8 It is the regeneration of the coenzyme by the copper substrate at different voltages in the test examples of the present invention;
[0042] Fig. 9 is the selectivity of the copper nanowire catalyst and the copper substrate to the coenzyme at different voltages in the test examples of the present invention;
[0043] Fig.10 It is a high-resolution transmission electron microscope of the copper nanowire catalyst of Example 1 of the present invention;
[0044] Fig.11 This is a comparison result of the selectivity and yield of the nickel-molybdenum catalyst of Example 1 and the copper nanowire catalyst of Example 1 for coenzyme regeneration. DETAILED DESCRIPTION
[0045] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0046] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0047] Example 1
[0048] This embodiment provides a method for preparing a copper-based catalyst, comprising the following steps:
[0049] Select size 1×1cm 2The copper substrate was immersed in a mixed solution containing 0.13M (NH4)2S2O8 and 2.6M KOH for 0.5h to obtain a substrate containing Cu(OH)2. Then, the substrate containing Cu(OH)2 was calcined at 300°C in an Ar atmosphere containing 5vol% H2 for 2h to obtain a substrate containing copper nanowires, and copper oxide existed on the surface of the copper nanowires. The substrate containing copper nanowires was electrochemically activated at a voltage of -1.2 to -0.7V, with a scan rate of 50mV / s, and a total of 60 cycles were scanned. A polycrystalline morphology was generated on the surface, and a polycrystalline copper nanowire catalyst was obtained, which was recorded as r-CuNWs. The height of the copper nanowire catalyst was 5-7μm and the diameter was 170-220nm.
[0050] Example 2
[0051] This embodiment provides a method for preparing a copper-based catalyst, comprising the following steps:
[0052] Select size 1×1cm 2 The copper substrate was immersed in a mixed solution containing 0.13M (NH4)2S2O8 and 2.6M KOH for 0.5h to obtain a substrate containing Cu(OH)2. The substrate containing Cu(OH)2 was then calcined at 200°C in an Ar atmosphere for 3h to obtain a substrate containing copper oxide nanowires. The substrate containing copper oxide nanowires was electrochemically activated at a voltage of -1.2 to -0.7V, with a scan rate of 50mV / s for a total of 60 cycles, and a polycrystalline morphology was generated on the surface to obtain a polycrystalline copper nanowire catalyst, denoted as r-CuNWs. The height of the copper nanowire catalyst was 6-8μm and the diameter was 150-200nm.
[0053] Example 3
[0054] This embodiment provides a method for preparing a copper-based catalyst, comprising the following steps:
[0055] Select size 1×1cm 2 The copper substrate was immersed in a mixed solution containing 0.13M (NH4)2S2O8 and 2.6M KOH for 0.5h to obtain a substrate containing Cu(OH)2. The substrate containing Cu(OH)2 was then calcined at 550°C in an Ar atmosphere for 3h to obtain a substrate containing cuprous oxide nanowires. The substrate containing cuprous oxide was electrochemically activated at a voltage of -1.2 to -0.7V, with a scan rate of 50mV / s for a total of 60 cycles. A polycrystalline morphology was generated on the surface, and a polycrystalline copper nanowire catalyst was obtained, which was recorded as r-CuNWs. The height of the copper nanowire catalyst was 5-8μm and the diameter was 190-230nm.
[0056] Comparative Example 1
[0057] This comparative example provides a method for preparing a copper-based catalyst, comprising the following steps:
[0058] First, 3g (NH4)2MoO4·4H2O, 300mg PVP, and 300mg NH4F were added to 90mL water. Then, the nickel foam was immersed in the above solution for 2h and shaken vigorously. The hydrothermal reaction was carried out at 150℃ for 6h. Finally, the Ni4Mo / MoO2 / NF electrocatalyst was obtained by calcining at 300℃ for 2h in an Ar atmosphere containing 5% H2.
[0059] Test example
[0060] This test example provides a performance test of a copper nanowire catalyst, as follows:
[0061] 1. Use copper substrate as the control group.
[0062] The copper nanowire catalyst and the copper substrate (respectively denoted as r-CuNWs and Cu foam) of Example 1 were used to react with the coenzyme NAD + Regeneration, at different times and with different NAD + The coenzyme regeneration performance was tested under different concentrations and voltages. The results are shown in the figure below.
[0063] (1) Coenzyme regeneration process: coenzyme NAD + The concentration was 2mmol / L. At -1.1V vs.Ag / AgCl, constant voltage electrolysis was performed for 40min. Samples were taken every 10min to test the conversion at different times.
[0064] Figures 1 to 3 The copper nanowire catalyst and copper substrate are used for coenzyme NAD + Regeneration, NAD at different times + conversion situation. Figure 1 NAD at different regeneration times + The concentration of Figure 2 is the 1,4-NADH obtained at different regeneration times, Figure 3 is the 1,6-NADH obtained at different regeneration times. Figures 1 to 3 It can be seen that the copper nanowire catalyst prepared by the present invention exhibits higher NAD + Conversion rate. Figure 1 It can be seen that the copper nanowire catalyst prepared by the present invention has an effect on the coenzyme NAD + During regeneration, most of the NAD + Reduced to NADH, regeneration time is short. Figures 2-3 It can be seen that the copper-based catalyst of the present invention can be used to convert most of the NAD +reduced to active 1,4-NADH, while the copper substrate converts most of the NAD + Reduced to inactive 1,6-NADH.
[0065] (2) Coenzyme regeneration process: voltage is -1.1V vs.Ag / AgCl, at different initial concentrations of coenzyme NAD +
[0066] (0.5mM, 2mM, 10mM) constant voltage electrolysis for 40min, testing different concentrations of coenzyme NAD + of regeneration.
[0067] Figures 4 to 6 The copper nanowire catalyst and copper substrate were used to generate the coenzyme NAD with different initial concentrations. + The regeneration test results. Figure 4 For different initial concentrations of coenzyme NAD + Regeneration under the action of copper nanowire catalyst, Figure 4 The others in the sentence refer to by-products. Figure 5 For different initial concentrations of coenzyme NAD + Regeneration under the action of copper substrate, Figure 6 For different initial concentrations of coenzyme NAD + , selectivity of copper nanowire catalysts and copper substrates. Figures 4-5 It can be seen that NAD + When the concentration is low, there is almost no byproduct, which shows that the copper nanowire catalyst and the copper substrate are effective for the low concentration of NAD + When the coenzyme concentration increases, especially at 10mM, the copper substrate produces more and more byproducts, such as NAD2, while the copper nanowire catalyst prepared by the present invention has almost no byproducts, and most of the products are 1,4-NADH, which shows that the copper nanowire catalyst of the present invention has a stronger ability to generate adsorbed hydrogen and has a better effect on coenzyme reduction. Figure 6 It can be seen that with the increase of coenzyme concentration, the by-products obtained from the copper substrate show an increasing trend, which further proves that the copper nanowire catalyst prepared by the present invention has a good coenzyme regeneration effect and has a stronger ability to generate adsorbed hydrogen.
[0068] from Figure 6 It can be seen that the copper nanowire catalyst of the present invention has higher selectivity, and most of the NAD + It is converted into NADH instead of NAD dimer (NAD2). The copper substrate produces a large amount of byproducts, such as NAD dimer, etc. This further shows that the copper nanocatalyst of the present invention has a higher adsorption hydrogen yield, making the hydrogenation process faster.
[0069] (3) Coenzyme regeneration process: NAD in coenzyme+ The concentration was 2mmol / L, and constant voltage electrolysis was performed for 40min at -1.2V, -1.1V, -1.0V, -0.9V, and -0.8V vs.Ag / AgCl, respectively, to test the conversion under different voltages.
[0070] Figure 7 The regeneration of coenzyme by copper nanowire catalyst under different voltages; Figure 8 The regeneration of coenzyme by copper substrate under different voltages; Fig. 9 The selectivity of copper nanowire catalyst and copper substrate for coenzyme under different voltages. Figures 7 to 9 It can be seen that compared with the copper substrate, the copper nanowire catalyst of the present invention shows a higher conversion rate, regeneration rate and selectivity of 1,4-NADH in a wider electrochemical window. As the potential increases, the regioselectivity or selectivity of the copper nanowire catalyst will increase. At -1.2Vvs.Ag / AgCl, only a few by-products appear. The high voltage improves the water dissociation ability, increases the active hydrogen, reduces the by-products, and improves the selectivity. Fig. 9 From the above, for copper substrate, when the applied potential increases from -0.8V to -1.2V, the selectivity increases from less than 30% to more than 65%, which can be explained by the increase in hydrogen evolution reaction (HER) kinetics, resulting in higher active hydrogen yield. The regional selectivity remains almost unchanged at around 75%, indicating that the hydrogenation site is independent of the potential change. Among them, Figure 7 and Figure 8 The curve in the figure corresponds to the right ordinate, and the bar chart corresponds to the left ordinate.
[0071] Fig.10 This is a high-resolution transmission electron microscopy of the copper nanowire catalyst in Example 1. It can be seen from the figure that there are a large number of grain boundaries on the surface of the copper nanowire catalyst, which are mainly formed between the (111) and (111) planes.
[0072] (4) Fig.11 The selectivity and yield of the nickel-molybdenum catalyst in comparative example 1 and the copper nanowire catalyst in example 1 for coenzyme regeneration are compared. Fig.11 The curve in the figure corresponds to the right ordinate, and the bar graph corresponds to the left ordinate. + The initial concentration of regeneration was 2 mM, and electrolysis was performed for 15 min at a voltage of -1.1 V vs. Ag / AgCl. It can be seen that the copper nanowire catalyst of the present invention shows a higher yield and selectivity of 1,4-NADH than the nickel-based catalyst.
[0073] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for preparing a copper-based catalyst for coenzyme regeneration, It is characterized in that The following steps are involved: (1) immersing a copper substrate in a functional solution to obtain a substrate containing nanowires; wherein the functional solution comprises an alkaline compound and an oxidant; (2) calcining and electrochemically activating the nanowire-containing substrate to obtain a copper nanowire catalyst.
2. The preparation method according to claim 1, It is characterized in that The height of the copper nanowire catalyst is 5 to 10 μm; and / or the diameter of the copper nanowire catalyst is 100 to 300 nm.
3. The preparation method according to claim 1 or 2, It is characterized in that The potential of the electrochemical activation is -1.2 to -0.7V.
4. The preparation method according to any one of claims 1 to 3, It is characterized in that The calcination temperature is 200-900° C. and the calcination time is 1-3 hours.
5. The preparation method according to claim 4, It is characterized in that The calcination atmosphere is a nitrogen-containing atmosphere, the calcination temperature is 200 to 400° C., and the calcination time is 1 to 3 hours; or, The calcination atmosphere is nitrogen or argon, the calcination temperature is 550-900°C, and the calcination time is 1-3h; or, The calcination atmosphere is a hydrogen-containing atmosphere, the calcination temperature is 300-500° C., and the calcination time is 1-3 hours.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that The alkaline compound is at least one of potassium hydroxide and sodium hydroxide; Preferably, the oxidant is (NH 4 ) 2 S 2 O 8 ; Preferably, the concentration of the alkaline compound in the functional solution is 1.3-2.6 mol / L, and the concentration of the oxidant is 0.0325-0.26 mol / L; Preferably, the molar ratio of the basic compound to the oxidant is 20:
1.
7. The copper-based catalyst prepared by the preparation method according to any one of claims 1 to 6.
8. A method for regenerating a coenzyme, It is characterized in that A copper-based catalyst prepared by the preparation method according to any one of claims 1 to 6.
9. The method according to claim 8, It is characterized in that The copper-based catalyst is used to electrochemically hydrogenate the coenzyme; Preferably, the voltage of the electrochemical reduction is -1.2 to -0.7 V; Preferably, the electrochemical reduction time is 20 to 30 minutes.
10. The method according to claim 8 or 9, It is characterized in that The coenzyme is NAD + and NADP + At least one of .