Acid environment-friendly anti-oxidation process for electrolytic copper foil
Through the acidic and environmentally friendly electrolytic copper foil anti-oxidation process, the composite anti-oxidation liquid and the electrolytic conditions are used to form a uniform thickness protective layer, which solves the problem of insufficient corrosion resistance and stability of copper foil in traditional methods, and achieves a higher Corrosion resistance and lower environmental impact.
Patent Information
- Application Number
- CN202410959197.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional copper foil anti-oxidation methods have limitations in improving corrosion resistance and stability, such as uneven thickness of the protective layer, low durability or high cost.
Using acidic and environmentally friendly electrolytic copper foil anti-oxidation process, the temperature and current density in the electrolytic cell are controlled to ensure a uniform electrolytic process by preparing a composite anti-oxidation liquid containing chromium trioxide, surfactant, pure water, preservative and citric acid. , form a protective layer of uniform thickness, and treat waste liquid through neutralizing agent to reduce environmental hazards.
It effectively improves the corrosion resistance and service life of the copper foil surface, provides a more stable and consistent protective effect, reduces environmental pollution, and improves product quality and consistency.
Smart Images

Figure CN118957704A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrolytic copper foil production, in particular to an acidic and environment-friendly anti-oxidation process for electrolytic copper foil. Background Art
[0002] Copper foil, as a key material in the electronics industry, is widely used in electronic devices such as printed circuit boards (PCBs). The surface quality of copper foil directly affects the performance and reliability of electronic devices. However, copper itself is easy to oxidize, especially in air and in environments with high humidity, and an oxide layer is easily formed on its surface, which affects its electrical conductivity and corrosion resistance. Traditional copper foil anti-oxidation methods mainly enhance its anti-oxidation properties through surface treatment or plating technology. However, these methods have certain limitations in improving the corrosion resistance and stability of copper foil. For example, the treated protective layer may have problems such as uneven thickness, low durability or high cost. For this reason, those skilled in the art have proposed an acidic and environmentally friendly anti-oxidation process for electrolytic copper foil to solve the above problems. Summary of the invention
[0003] In view of the shortcomings of the prior art, the present invention provides an acidic and environmentally friendly anti-oxidation process for electrolytic copper foil, which solves the problems of low corrosion resistance and stability of the electrolytic copper foil in the prior art.
[0004] To achieve the above objectives, the present invention is implemented by the following technical scheme: an acidic and environmentally friendly anti-oxidation process for electrolytic copper foil, comprising the following steps:
[0005] S1. Prepare a composite anti-oxidation liquid, which contains chromium trioxide, surfactant, pure water, preservative, citric acid and other substances;
[0006] S2. Prepare an electrolytic cell of suitable size and ensure that the temperature and current density can be controlled. Then add the pre-prepared anti-oxidation liquid into the electrolytic cell and start the stirring or circulation equipment to ensure the uniformity of the liquid.
[0007] S3. Clean the surface of the copper foil to ensure there is no oil, oxide or other contaminants;
[0008] S4, completely immerse the clean copper foil in the anti-oxidation solution in the electrolytic tank, start the power supply, apply appropriate current density and set electrolysis time, and start the electrolysis process;
[0009] S5. During the electrolysis process, monitor the temperature and pH value of the electrolyte to ensure that these parameters remain within a stable range, and adjust the current density according to the process requirements to ensure that a uniform and appropriately thick oxide layer is formed on the surface of the copper foil;
[0010] S6. After the electrolytic treatment is completed, the copper foil is removed and immediately rinsed thoroughly with clean water or salt water to remove the residual anti-oxidation liquid. A neutralizer is used to neutralize the residual acid electrolyte to ensure that the waste liquid meets environmental protection requirements.
[0011] Preferably, the step S1 of preparing the composite anti-oxidation liquid comprises the following steps:
[0012] S101. In a clean container, add an appropriate amount of pure water, and according to the formula, slowly add chromium trioxide into the pure water while stirring to ensure that the chromium trioxide is evenly dispersed;
[0013] S102, adding an appropriate amount of surfactant, continuing to stir until completely dissolved and mixed, then adding citric acid, and adjusting the pH value of the solution as needed;
[0014] S103, add an appropriate amount of preservative to ensure the stability of the anti-oxidation liquid and its long-term shelf life.
[0015] Preferably, the amount of chromium trioxide added is 0.5% to 5% of the dilution liquid, and the preservative is one or a combination of methylparahydroxybenzoic acid, ethylparahydroxybenzoate, and sodium acetate.
[0016] Preferably, the pH of the solution in step S102 is between 2.4 and 3.2.
[0017] Preferably, the S2 step specifically includes the following steps:
[0018] S201. Select an electrolytic cell suitable for the work. Its size and shape should be determined according to the workload and material size. Ensure that the internal surface of the electrolytic cell is clean and free of oil or other impurities;
[0019] S202. If temperature control is required, ensure that the ambient temperature around the electrolytic cell is stable, or use the built-in heating or cooling equipment of the electrolytic cell to set and maintain the appropriate operating temperature to ensure the stability and consistency of the process;
[0020] S203, according to the material requirements and the composition of the anti-oxidation solution, setting an appropriate current density, which is achieved by adjusting the shape and spacing of the electrodes in the electrolytic cell, and the current output of the power supply;
[0021] S204, slowly and evenly adding the pre-prepared anti-oxidation liquid into the electrolytic cell to avoid violent stirring or rapid injection, so as to prevent the generation of bubbles and fluctuations of the liquid;
[0022] S205, start the agitator inside the electrolytic cell to ensure that the anti-oxidation liquid is fully mixed and evenly distributed in the entire electrolytic cell.
[0023] Preferably, in step S205, the stirring speed of the stirrer is 100-200 r / min, the humidity is adjusted to 30-50%, the temperature is controlled at 80-100° C., and the stirring time is 40-80 min.
[0024] Preferably, the electrolysis time in step S4 is 5-45 min, and the current density can be 0.1 A / m 2 To 1A / m 2 .
[0025] Preferably, the neutralizing agent is one or a combination of sodium bicarbonate, sodium carbonate and sodium hydroxide.
[0026] The present invention provides an acidic and environmentally friendly anti-oxidation process for electrolytic copper foil, which has the following beneficial effects:
[0027] 1. The present invention adds a step of configuring a composite anti-oxidation liquid in the electrolytic copper foil anti-oxidation process. The composite anti-oxidation liquid can be combined with a variety of chemical substances to improve the quality and stability of the formed protective layer, thereby effectively reducing the oxidation rate of the copper foil surface, extending its service life and improving its corrosion resistance under different environmental conditions. At the same time, the composite anti-oxidation liquid can provide a more stable and consistent protection effect, which helps to improve the quality stability and consistency of the product.
[0028] 2. After the electrolytic treatment is completed, the present invention takes out the copper foil, removes the residual anti-oxidation liquid, and uses a neutralizer to neutralize the acidic components in the acidic solution into a neutral or nearly neutral aqueous solution, thereby reducing its harm to the environment. The overall preparation engineering design is reasonable and the anti-oxidation effect of the electrolytic copper foil is good.
[0029] 3. The present invention can adjust the reaction rate and covering performance of the anti-oxidation liquid by controlling the temperature and current density in the electrolytic cell. At the same time, the anti-oxidation liquid can be ensured to be evenly distributed in the electrolytic cell by stirring, ensuring that each copper foil surface is treated in the same way to form a consistent protective layer. The improvement in uniformity can reduce batch differences that may occur in production, thereby improving the quality stability and consistency of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1: Application of environmentally friendly acidic anti-oxidation process for electrolytic copper foil
[0033] Specific steps:
[0034] S1. Preparation of composite anti-oxidation liquid:
[0035] Chromium trioxide, surfactant, pure water, preservative and citric acid are selected and prepared into a composite anti-oxidation liquid in a specific ratio.
[0036] S2. Electrolytic cell preparation and liquid uniformity:
[0037] Select an electrolytic cell of appropriate size and ensure that the temperature and current density can be controlled. Pour the pre-prepared anti-oxidation solution into the electrolytic cell and start the stirring or circulation equipment to ensure the uniformity of the liquid.
[0038] S3. Copper foil surface cleaning:
[0039] Clean the copper foil surface thoroughly to ensure there is no oil, oxide or other contaminants.
[0040] S4. Copper foil electrolytic treatment:
[0041] Completely immerse the clean copper foil in the anti-oxidation solution in the electrolytic tank, start the power supply and apply appropriate current density and set electrolysis time to start the electrolysis process.
[0042] Test 1: Comparison of anti-oxidation effects
[0043] Experimental setup:
[0044] Two groups of electrolytic cells were set up, each using the same electrolytic copper foil surface area.
[0045] Processing materials:
[0046] One group used traditional anti-oxidation liquid, and the other group used the above-mentioned composite anti-oxidation liquid.
[0047] Electrolysis conditions:
[0048] The current density and electrolysis time were set to be the same.
[0049] Experimental data table:
[0050]
[0051] Example 2: Evaluation of the application advantages of electrolytic copper foil acidic environmentally friendly anti-oxidation process
[0052] Specific steps:
[0053] S5. Sample preparation before performance evaluation:
[0054] Take out the treated copper foil samples from each electrolytic cell to ensure that the sample surface is clean and free of contamination.
[0055] S6. Performance evaluation test:
[0056] Using appropriate test methods and instruments, perform the following tests on each set of copper foil samples:
[0057] Corrosion resistance test: The copper foil samples are exposed to a simulated corrosion environment to observe the stability and corrosion resistance of the surface oxide layer.
[0058] Electrochemical performance test: measure the electrochemical properties of the sample, such as resistivity, electrode potential, etc., to evaluate the effect of the anti-oxidation solution on the electrical properties of the copper foil.
[0059] S7. Data analysis and comparison:
[0060] Collect and analyze all data and test results obtained in Example 1 and Example 2. Compare the differences between the composite anti-oxidation liquid and the traditional anti-oxidation liquid in terms of protection effect, stability and cost-effectiveness.
[0061] Experimental column 2: Analysis of electrolyte pH and temperature changes
[0062] Experimental setup:
[0063] The pH and temperature changes in the electrolyte were monitored to evaluate the stability and influencing factors of the environmental conditions during the electrolysis process.
[0064] Time Node:
[0065] The pH value and temperature of the electrolyte were continuously recorded every hour after the start of electrolysis.
[0066] Experimental data table:
[0067] Time point (hour) pH Temperature(℃) 0 5.5 25 1 5.3 26 2 5.1 27 4 5.0 28 6 4.9 29
[0068] Experimental results analysis:
[0069] Based on the collected data, analyze the trends of electrolyte pH and temperature changes, evaluate the potential impact of these changes on the electrolysis process and anti-oxidation effect, and propose necessary adjustment suggestions or optimization plans to improve process stability and product quality.
[0070] Implementation 3: Process Optimization and Continuous Improvement
[0071] Specific steps:
[0072] S8. Process optimization scheme design:
[0073] Based on the data analysis results of Implementation 1 and Implementation 2, process optimization suggestions for composite anti-oxidation liquid are proposed. Considerations include but are not limited to the following aspects:
[0074] Adjust the temperature control and stirring equipment of the electrolytic cell to improve the uniformity of the anti-oxidation solution.
[0075] Optimize the current density and electrolysis time during the electrolysis process to achieve better protection effect.
[0076] Consider using alternative, more environmentally friendly raw materials or adjusting formulations to reduce costs and environmental impact.
[0077] S9. Implement optimization plan:
[0078] Implement the design optimization plan in a laboratory scale or small-scale production environment. Record and analyze the anti-oxidation effect and other performance indicators of copper foil under new process conditions.
[0079] S10. Continuous Improvement and Feedback:
[0080] Regularly collect actual operating data under new process conditions. Evaluate the actual effect of the optimization plan by comparing it with the initial expectations of the experimental design. Based on the experimental results, continuously improve the process details and feed back into the process optimization plan to ensure continuous improvement of product quality and process stability.
[0081] Test series 3: long-term stability evaluation
[0082] Experimental setup:
[0083] Long-term monitoring of the protective effect of the composite anti-oxidation liquid and the stability of the electrolyte performance in a production environment.
[0084] Time Node:
[0085] Record weekly or monthly for at least half a year or longer.
[0086] Experimental data record:
[0087] The oxide layer thickness, surface uniformity and electrochemical performance indicators of copper foil samples were measured regularly.
[0088] Regularly monitor the electrolyte pH, temperature changes, and any other relevant parameters.
[0089] Experimental results analysis:
[0090] Analyze the data collected during the long-term experiment to evaluate the long-term stability and continuous protection effect of the composite anti-oxidation liquid in actual production. Based on the analysis results, make further suggestions for improvement or adjustment of process parameters to ensure continuous improvement of product quality and process stability.
[0091] Implementation Column 4: Expanded Application and Market Promotion
[0092] Specific steps:
[0093] S11. Market demand analysis:
[0094] Research the market to understand the potential application demand of composite anti-oxidation liquid in the electronics, automobile and other industries. Evaluate the market's acceptance and demand for efficient and environmentally friendly anti-oxidation processes.
[0095] S12. Product Adaptation and Standardization:
[0096] According to market demand, adjust the formula or process parameters of the composite anti-oxidation liquid to ensure that it meets the specific requirements of different industries. Formulate relevant product standards and specifications to ensure product quality and consistency.
[0097] S13. Promotion and sales:
[0098] Formulate marketing strategies, including exhibitions, technical seminars, media publicity, etc., to show potential customers the advantages and application effects of composite anti-oxidation liquid. Establish sales channels, establish cooperative relationships with major industry players, and promote product marketing and sales.
[0099] Test column 4: Comparative analysis of competing products
[0100] Experimental setup:
[0101] Select several mainstream or competitive antioxidant fluid products and conduct comparative tests in a laboratory or small-scale production environment.
[0102] Time Node:
[0103] Depending on the progress of the experiment, comparative tests will be conducted monthly or quarterly.
[0104] Experimental data record:
[0105] Comparative measurement of the oxide layer thickness, surface uniformity, electrochemical properties and other indicators of copper foil samples in competitor anti-oxidation liquid and composite anti-oxidation liquid.
[0106] Record and analyze the advantages and disadvantages of different antioxidant solutions under experimental conditions.
[0107] Experimental results analysis:
[0108] Analyze the data of competitive product comparison experiments to evaluate the differences between the composite antioxidant liquid and competitive products in terms of protection effect, cost-effectiveness, environmental friendliness, etc. Adjust the marketing strategy or product optimization plan based on the analysis results to enhance the competitive advantage and wide application of the composite antioxidant liquid in the market.
[0109] The above are the details of Implementation Column 4 and Experimental Column 4, which aim to further promote the application of composite antioxidant liquid and enhance its market competitiveness through market promotion and competitive product comparison analysis.
[0110] In summary: the present invention adds the step of configuring a composite anti-oxidation liquid in the electrolytic copper foil anti-oxidation process. The composite anti-oxidation liquid can be combined with a variety of chemical substances to improve the quality and stability of the formed protective layer, thereby effectively reducing the oxidation rate of the copper foil surface, extending its service life and improving its corrosion resistance under different environmental conditions. At the same time, the composite anti-oxidation liquid can provide a more stable and consistent protection effect, which helps to improve the quality stability and consistency of the product.
[0111] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An acidic and environmentally friendly anti-oxidation process for electrolytic copper foil, characterized in that: The following steps are involved: S1. preparing a composite anti-oxidation liquid, which comprises chromium trioxide, a surfactant, pure water, a preservative, citric acid and other substances; S2. Prepare an electrolytic cell of suitable size and ensure that the temperature and current density can be controlled. Then add the pre-prepared anti-oxidation liquid into the electrolytic cell and start the stirring or circulation equipment to ensure the uniformity of the liquid. S3. Clean the surface of the copper foil to ensure there is no oil, oxide or other contaminants; S4, completely immerse the clean copper foil in the anti-oxidation solution in the electrolytic tank, start the power supply, apply appropriate current density and set electrolysis time, and start the electrolysis process; S5. During the electrolysis process, monitor the temperature and pH value of the electrolyte to ensure that these parameters remain within a stable range, and adjust the current density according to the process requirements to ensure that a uniform and appropriately thick oxide layer is formed on the surface of the copper foil; S6. After the electrolytic treatment is completed, the copper foil is removed and immediately rinsed thoroughly with clean water or salt water to remove the residual anti-oxidation liquid. A neutralizer is used to neutralize the residual acid electrolyte to ensure that the waste liquid meets environmental protection requirements.
2. The acidic and environmentally friendly anti-oxidation process for electrolytic copper foil according to claim 1, characterized in that: The S1 preparation of the composite anti-oxidation liquid comprises the following steps: S101. In a clean container, add an appropriate amount of pure water, and according to the formula, slowly add chromium trioxide into the pure water while stirring to ensure that the chromium trioxide is evenly dispersed; S102, adding an appropriate amount of surfactant, continuing to stir until completely dissolved and mixed, then adding citric acid, and adjusting the pH value of the solution as needed; S103, add an appropriate amount of preservative to ensure the stability of the anti-oxidation liquid and its shelf life for long-term use.
3. The acidic and environmentally friendly anti-oxidation process for electrolytic copper foil according to claim 1, characterized in that: The amount of chromium trioxide added is 0.5% to 5% of the dilution liquid, and the preservative is one or a combination of methylparahydroxybenzoic acid, ethylparahydroxybenzoate, and sodium acetate.
4. The acidic and environmentally friendly anti-oxidation process for electrolytic copper foil according to claim 1, characterized in that: The pH of the solution in step S102 is between 2.4 and 3.
2.
5. The acidic and environmentally friendly anti-oxidation process for electrolytic copper foil according to claim 1, characterized in that: The S2 step specifically includes the following steps: S201. Select an electrolytic cell suitable for the work. Its size and shape should be determined according to the workload and material size. Ensure that the internal surface of the electrolytic cell is clean and free of oil or other impurities; S202. If temperature control is required, ensure that the ambient temperature around the electrolytic cell is stable, or use the built-in heating or cooling equipment of the electrolytic cell to set and maintain the appropriate operating temperature to ensure the stability and consistency of the process; S203, according to the material requirements and the composition of the anti-oxidation solution, setting an appropriate current density, which is achieved by adjusting the shape and spacing of the electrodes in the electrolytic cell, and the current output of the power supply; S204, slowly and evenly adding the pre-prepared anti-oxidation liquid into the electrolytic cell to avoid violent stirring or rapid injection, so as to prevent the generation of bubbles and fluctuations of the liquid; S205, start the agitator inside the electrolytic cell to ensure that the anti-oxidation liquid is fully mixed and evenly distributed in the entire electrolytic cell.
6. The acidic and environmentally friendly anti-oxidation process for electrolytic copper foil according to claim 5, characterized in that: In the step S205, the stirring speed of the stirrer is 100-200 r / min, the humidity is adjusted to 30-50%, the temperature is controlled at 80-100° C., and the stirring time is 40-80 min.
7. The acidic and environmentally friendly anti-oxidation process for electrolytic copper foil according to claim 1, characterized in that: The electrolysis time in step S4 is 5-45 min, and the current density can be 0.1 A / m 2 To 1A / m 2 .
8. The acidic and environmentally friendly anti-oxidation process for electrolytic copper foil according to claim 1, characterized in that: The neutralizing agent is one or a combination of sodium bicarbonate, sodium carbonate and sodium hydroxide.
Citation Information
Cited By
Cooling method and device for shape memory alloy driver
CN119486073A