Monocrystal 1, 8-diamino octane lead iodide molecular ferroelectric crystal and preparation and application thereof
The single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal was prepared by hydrothermal method, which solved the problem of insufficient ferroelectricity of two-dimensional layered lead-based compounds in the prior art, and achieved high purity and high crystallization The preparation of materials of the degree of material has expanded its application prospects in the fields of photoelectric and ferroelectricity.
Patent Information
- Application Number
- CN202411011807.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the ferroelectricity performance in two-dimensional layered lead-based organic and inorganic hybrid compounds is not obvious, and the lack of single crystalline materials with high crystallinity and high purity limits its application in the field of ferroelectric photovoltaics.
The single crystal 1,8-diaminooctane lead iodide molecule ferroelectric crystal was prepared by hydrothermal method. The PbI2 solution was mixed with 1,8-diaminooctane and hydrothermal reaction was carried out, washing and drying, forming Two-dimensional layered structure with intrinsic ferroelectricity.
Successfully prepared single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal with high crystallinity and purity, with clear structure and stable properties, suitable for photodetectors, data storage, optoelectronic devices and iron Electric photovoltaics and other fields.
Smart Images

Figure CN118957762A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of molecular ferroelectrics, and in particular to a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal and preparation and application thereof. Background Art
[0002] In the past few decades, inorganic ceramic ferroelectrics have been widely used due to their excellent electrical and optical properties, such as BaTiO3, BiFeO3, etc. Until recently, in order to solve the increasingly severe environmental, energy and cost problems brought by ceramic ferroelectrics, organic-inorganic hybrid molecular ferroelectrics with perovskite or perovskite-related crystal structures have attracted widespread attention as promising candidate materials in the fields of flexible sensors, non-volatile memories, optoelectronic devices, ferroelectric photovoltaics, etc. Among them, organic-inorganic hybrid lead-based molecular ferroelectrics are particularly interesting in optoelectronic applications due to their structural diversity, excellent charge transport, superior stability and natural quantum well effect. Lead-based halide solar cells represented by CH3NH3PbI3 have amazing power conversion efficiencies (PCEs) increased from 3.8% to 25.7% through methods such as component substitution, device structure optimization and defect passivation. However, whether there is intrinsic ferroelectricity in these compounds remains inconclusive. Therefore, organic-inorganic hybrid lead-based molecular ferroelectrics with intrinsic ferroelectricity will become a research hotspot in the field of ferroelectric photovoltaics. Compared with three-dimensional (3D) organic-inorganic hybrid lead-based molecular ferroelectrics, two-dimensional (2D) species show higher structural tolerance without the length restriction of interlayer organic cations, thus bringing unlimited possibilities for material design and exploration. Although many two-dimensional layered lead-based hybrid organic-inorganic compounds have been reported to date, only a few cases exhibit ferroelectricity.
[0003] Therefore, finding new designs and new structures, preparing high-crystallinity, high-purity organic-inorganic hybrid lead-based molecular ferroelectric single crystals, and studying their properties are of great significance both from the perspective of basic research and from the perspective of performance and application. Summary of the invention
[0004] In order to solve the above problems, the purpose of the present invention is to provide a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal and its preparation and application. The single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal of the present invention has intrinsic ferroelectricity.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] The first object of the present invention is to provide a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal, the chemical formula of which is C8N2H 22 PbI4, whose unit cell parameters are and α=90°, β=106.823(6)°, γ=90°.
[0007] The second object of the present invention is to provide a method for preparing a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal, comprising the following steps:
[0008] (S1) mixing the PbI2 solution and 1,8-diaminooctane to obtain a mixed solution;
[0009] (S2) subjecting the mixed solution obtained in step (S1) to a hydrothermal reaction, and then washing and drying the product in sequence to obtain a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal.
[0010] In one embodiment of the present invention, in step (S1), the PbI2 solution is a mixture of PbI2 and HI (mass fraction is 50%).
[0011] In one embodiment of the present invention, the usage ratio of PbI2 to HI is 1 mmol: 3-5 mL.
[0012] In one embodiment of the present invention, in step (S1), the molar ratio of PbI2 solution to 1,8-diaminooctane is 1:0.8-1.2.
[0013] In one embodiment of the present invention, the molar ratio of the PbI2 solution to the 1,8-diaminooctane is 1:1.
[0014] In one embodiment of the present invention, in step (S2), during the hydrothermal reaction, the temperature is 100-160° C. and the time is 8-12 hours.
[0015] In one embodiment of the present invention, in step (S2), during the washing process, the detergent is selected from one or both of ethyl acetate and n-butane.
[0016] In one embodiment of the present invention, in step (S2), the temperature during the drying process is 55-70°C.
[0017] The third object of the present invention is to provide a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal for use in photoelectric detectors, data storage, optoelectronic devices or ferroelectric photovoltaic fields.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The present invention adopts a mild and simple hydrothermal method to prepare single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystals. The sample prepared by the hydrothermal method has good quality and a relatively regular morphology.
[0020] (2) The single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal structure provided by the present invention is clear, and the PbI6 octahedral layer and (C8N2H 22 ) 2+ The cation layer can be infinitely staggered to form a two-dimensional layered structure, has stable properties, and has unique single crystal spectrum information, which has a clearer direction for studying the properties of the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal; and the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal provided by the present invention has broad application prospects in the fields of photoelectric detectors, data storage, optoelectronic devices, ferroelectric photovoltaics, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is the XRD spectrum of the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal in Example 1;
[0022] Figure 2 is a structural diagram of the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal in Example 1;
[0023] Figure 3 This is an optical micrograph of the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal in Example 1;
[0024] Figure 4 is the absorption band gap spectrum of the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal in Example 1;
[0025] Figure 5 This is the IT curve of the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal in Example 1. DETAILED DESCRIPTION
[0026] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0027] In the following examples, unless otherwise specified, all reagents used are commercially available reagents, and all detection means and methods used are conventional detection means and methods in the art.
[0028] Example 1
[0029] This embodiment provides a hydrothermal synthesis method of a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal, which specifically includes the following steps:
[0030] (S1) dissolving 0.01 mol of PbI2 in 60 mL of hydroiodic acid and mixing by magnetic stirring to obtain a PbI2 solution;
[0031] (S2) After all the components are dissolved, 0.01 mol of 1,8-diaminooctane is added to the above solution, and magnetic stirring is continued until the solution becomes viscous and yellow to obtain a mixed solution;
[0032] (S3) The mixed solution obtained in step (S2) is loaded into a 100mL reactor liner, and the reactor is loaded, and it is placed flat and tightened. After reacting in a 120°C oven for 12 hours, the reactor is cooled to room temperature and the pressure is released; after the reactor is cooled and the pressure is released, the supernatant is slowly poured out, and the yellow precipitate is retained. The precipitate is transferred to a 50mL large centrifuge tube with the assistance of a disposable pipette, and ethyl acetate is sucked with a pipette to centrifuge and wash the crystal sample, and it is careful not to contaminate the ethyl acetate reagent; the yellow sample is repeatedly centrifuged, and the upper layer of liquid is poured out after each centrifugation, and the precipitate is retained, and the previous step is repeated to add ethyl acetate to continue washing until the solvent is transparent after centrifugation; the above-washed yellow precipitate is dried in a drying oven at 60°C to obtain a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal.
[0033] After testing, the size of the single crystal product is about 100 microns, and the chemical formula of the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal is C8N2H 22 PbI4.
[0034] Performance Test:
[0035] Crystal data of the yellow single crystal obtained in Example 1 were collected using a Bruker D8 single crystal diffractometer in ω scanning mode under Mo-Kα (λ=0.71073A) radiation at 296K. As shown in Table 1, the crystal is monoclinic, with a space group of Pc, α=90°, β=106.823(6)°, γ=90°; Z=2,
[0036] Table 1 Crystal parameters of 1,8-diaminooctane lead iodide molecular ferroelectric single crystal
[0037]
[0038] The single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal prepared in Example 1 was detected by an X-ray diffractometer, and its XRD pattern was as follows: Figure 1 As shown, through Figure 1 It can be found that the experimentally obtained XRD pattern is in good agreement with the simulated data based on the crystal structure, indicating that the obtained sample is phase-pure and has a high degree of crystallinity.
[0039] The results of single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystals are as follows Figure 2 As shown, through Figure 2 It can be found that, in terms of structure, the central Pb 2+ cation with four separate and two adjacent bridging I - The anion coordinates to form a PbI6 octahedron, and the PbI6 octahedron layer is connected with (C8N2H 22 )2+ The cation layers allow for infinite interlacing to form a two-dimensional layered structure.
[0040] The crystal morphology of the yellow single crystal obtained in Example 1 was characterized. Figure 3 As shown, through Figure 3 It can be found that the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal prepared in this embodiment has a regular polyhedral morphology.
[0041] The prepared molecular ferroelectric C8N2H was characterized by UV-visible-near-infrared spectrophotometer. 22 The PbI4 powder was subjected to absorption tests, such as Figure 4 As shown, through Figure 4 It can be found that the band gap of single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal is 2.36eV.
[0042] The photoelectric properties of the prepared molecular ferroelectric materials were tested using a KEITHLEY 2450 Source Meter. Figure 5 As shown, through Figure 5 It can be found that the direction of the photocurrent can be changed by adjusting the direction of the polarization voltage, indicating that the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal prepared in this embodiment has obvious ferroelectric photovoltaic properties and can be applied to photodetectors, data storage, optoelectronic devices or ferroelectric photovoltaic fields.
[0043] Example 2
[0044] This embodiment provides a hydrothermal synthesis method of a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal, which specifically includes the following steps:
[0045] (S1) dissolving 0.01 mol of PbI2 in 60 mL of hydroiodic acid and mixing by magnetic stirring to obtain a PbI2 solution;
[0046] (S2) After all the components are dissolved, 0.01 mol of 1,8-diaminooctane is added to the above solution, and magnetic stirring is continued until the solution becomes viscous and yellow to obtain a mixed solution;
[0047] (S3) The mixed solution obtained in step (S2) is loaded into a 100 mL reactor liner, and the reactor is loaded, and it is placed flat and tightened. After reacting in a 110° C. oven for 10 hours, the reactor is cooled to room temperature and the pressure is released; after the reactor is cooled and the pressure is released, the supernatant is slowly poured out, and the yellow precipitate is retained. The precipitate is transferred to a 50 mL large centrifuge tube with the assistance of a disposable pipette, and ethyl acetate is taken with a pipette to centrifuge and wash the crystal sample, and it is careful not to contaminate the ethyl acetate reagent; the yellow sample is repeatedly centrifuged, and the upper layer of liquid is poured out after each centrifugation, and the precipitate is retained, and the previous step is repeated to add ethyl acetate to continue washing until the solvent is transparent after centrifugation; the above-washed yellow precipitate is dried in a drying oven at 60° C. to obtain a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal.
[0048] After testing, the size of the single crystal product is about 70 microns, and the chemical formula of the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal is C8N2H 22 PbI4.
[0049] Example 3
[0050] This embodiment provides a hydrothermal synthesis method of a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal, which specifically includes the following steps:
[0051] (S1) dissolving 0.01 mol of PbI2 in 60 mL of hydroiodic acid and mixing by magnetic stirring to obtain a PbI2 solution;
[0052] (S2) After all the components are dissolved, 0.01 mol of 1,8-diaminooctane is added to the above solution, and magnetic stirring is continued until the solution becomes viscous and yellow to obtain a mixed solution;
[0053] (S3) The mixed solution obtained in step (S2) is loaded into a 100mL reactor liner, and the reactor is loaded. It is important to lay it flat and tighten it. After reacting in a 100°C oven for 8 hours, the reactor is cooled to room temperature and the pressure is released. After the reactor is cooled and the pressure is released, the supernatant is slowly poured out, and the yellow precipitate is retained. The precipitate is transferred to a 50mL large centrifuge tube with the assistance of a disposable pipette, and ethyl acetate is taken with a pipette to centrifuge and wash the crystal sample, and it is important not to contaminate the ethyl acetate reagent; the yellow sample is repeatedly centrifuged, and the upper layer of liquid is poured out after each centrifugation, and the precipitate is retained. The previous step is repeated to add ethyl acetate for further washing until the solvent is transparent after centrifugation; the above-washed yellow precipitate is dried in a drying oven at 60°C to obtain a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal.
[0054] After testing, the size of the single crystal product is about 40 microns, and the chemical formula of the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal is C8N2H 22 PbI4.
[0055] Comparative Example 1
[0056] The difference between this comparative example and Example 1 is that the washing reagent is different, and specifically comprises the following steps:
[0057] (S1) dissolving 0.01 mol of PbI2 in 60 mL of hydroiodic acid and mixing by magnetic stirring to obtain a PbI2 solution;
[0058] (S2) After all the components are dissolved, 0.01 mol of 1,8-diaminooctane is added to the above solution, and magnetic stirring is continued until the solution becomes viscous and yellow to obtain a mixed solution;
[0059] (S3) The mixed solution obtained in step (S2) is loaded into a 100mL reactor liner, and the reactor is loaded. It is important to lay it flat and tighten it. After reacting in a 120°C oven for 12 hours, the reactor is cooled to room temperature and the pressure is released. After the reactor is cooled and the pressure is released, the supernatant is slowly poured out, and the yellow precipitate is retained. The precipitate is transferred to a 50mL large centrifuge tube with the aid of a disposable pipette. Deionized water is drawn with a pipette to centrifuge and wash the crystal sample. It is found that the product is completely dissolved in deionized water, and no crystals can be obtained. This is because the crystals are extremely soluble in deionized water. Therefore, special attention should be paid to the washing method of the crystals, especially deionized water cannot be used for washing.
[0060] Comparative Example 2
[0061] This comparative example is different from Example 1 in that the molar ratio of PbI2 to 1,8-diaminooctane is different, and specifically comprises the following steps:
[0062] (S1) dissolving 0.01 mol of PbI2 in 60 mL of hydroiodic acid and mixing by magnetic stirring to obtain a PbI2 solution;
[0063] (S2) After all the components are dissolved, 0.001 mol of 1,8-diaminooctane is added to the above solution, and magnetic stirring is continued until the solution becomes viscous and yellow to obtain a mixed solution;
[0064] (S3) The mixed solution obtained in step (S2) is loaded into a 100 mL reactor liner, and the reactor is loaded, and it is made to be flat and tightened. After reacting in an oven at 120°C for 12 hours, the reactor is cooled to room temperature and the pressure is released. After the reactor is cooled and the pressure is released, almost no precipitation is produced and no crystals can be obtained. This is because the content of 1,8-diaminooctane is too low and the content of necessary reactants is insufficient, resulting in the inability to generate the required crystals.
[0065] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the explanation of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal, It is characterized in that Its chemical formula is C 8 N 2 H 22 PbI 4 , whose unit cell parameters are and α=90°, β=106.823(6)°, γ=90°.
2. A method for preparing the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal as claimed in claim 1, It is characterized in that The following steps are involved: (S1) PbI 2 The solution is mixed with 1,8-diaminooctane to obtain a mixed solution; (S2) subjecting the mixed solution obtained in step (S1) to a hydrothermal reaction, and then washing and drying the product in sequence to obtain a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal.
3. A method for preparing a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal according to claim 2, It is characterized in that In step (S1), the PbI 2 Solution is PbI 2 Mixture with HI.
4. A method for preparing a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal according to claim 3, It is characterized in that PbI 2 The dosage ratio of HI is 1mmol:3~5mL.
5. A method for preparing a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal according to claim 2, It is characterized in that In step (S1), PbI 2 The molar ratio of the solution to 1,8-diaminooctane is 1:0.8-1.
2.
6. A method for preparing a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal according to claim 5, It is characterized in that PbI 2 The molar ratio of the solution to 1,8-diaminooctane is 1:
1.
7. A method for preparing a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal according to claim 2, It is characterized in that In step (S2), during the hydrothermal reaction, the temperature is 100-160° C. and the time is 8-12 hours.
8. A method for preparing a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal according to claim 2, It is characterized in that In step (S2), during the washing process, the detergent is selected from one or both of ethyl acetate and n-butane.
9. A method for preparing a single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal according to claim 2, It is characterized in that In step (S2), during the drying process, the temperature is 55-70°C.
10. An application of the single crystal 1,8-diaminooctane lead iodide molecular ferroelectric crystal as claimed in claim 1 in the fields of photodetectors, data storage, optoelectronic devices or ferroelectric photovoltaics.