Polyacrylonitrile precursor, polyacrylonitrile-based carbon fiber and preparation method thereof
By adjusting the polymerization formula and process parameters, polyacrylonitrile-based carbon fibers with small tow specifications and thin single filament diameters were prepared, which solved the problem that it was difficult to meet the needs of high precision, ultra-thin and ultra-fine applications in the prior art, and achieved high efficiency , simplified preparation process.
Patent Information
- Application Number
- CN202411234891.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-15
AI Technical Summary
It is difficult to prepare polyacrylonitrile-based carbon fibers with small tow specifications and thin single filament diameters in the prior art, which cannot meet the needs of high-precision, ultra-thin and ultra-fine application scenarios.
By adjusting the polymerization formula and preparation process, the content of comonomers is increased, and the finer spinning hole diameter and larger pore spacing are used to simplify the spinning process, including first-stage solidification bath, six-stage hot water drafting, first-stage upper Oil and first-stage drying densification treatment reduces pre-oxidation treatment time and ensures the homogeneity and orientation of the fibers.
The preparation of polyacrylonitrile raw wire and polyacrylonitrile-based carbon fibers with small tow specifications and thin single filament diameters has been achieved, which improves the tensile strength and tensile modulus of the fibers, simplifies the preparation process, and improves production efficiency.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of carbon fibers, and in particular to a polyacrylonitrile precursor, a polyacrylonitrile-based carbon fiber and a preparation method thereof. Background Art
[0002] Polyacrylonitrile (PAN)-based carbon fiber is a high-tech integrated, high-value-added product with properties such as light weight, high strength, high temperature resistance and corrosion resistance. It has been widely used in aerospace, aviation and industrial supplies.
[0003] At present, the preparation of polyacrylonitrile-based carbon fiber is mainly as follows: spinning polyacrylonitrile spinning solution (spinning, coagulation molding, water washing, hot water drawing, oiling, drying and densification, steam drawing and relaxation heat setting) to obtain polyacrylonitrile precursor (also known as the precursor of polyacrylonitrile-based carbon fiber); then pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment are performed on the polyacrylonitrile precursor to obtain polyacrylonitrile-based carbon fiber. At present, the tow K number of polyacrylonitrile-based carbon fiber prepared in the prior art is ≥1K, and the single fiber diameter is 4.7-7μm.
[0004] However, the domestic manufacturing industry is transforming to high-end, and various special applications require special-shaped, ultra-thin, and ultra-fine structures, which poses higher challenges to the upgrading and development of new materials. In view of the urgent demand for special fibers in high-precision, ultra-thin, and ultra-fine applications in special fields (such as micro-satellites, micro-drones, ultra-thin and ultra-large panels, and high-precision medical devices), the development of a new generation of carbon fibers with small tow specifications and fine monofilament diameters has become an important direction.
[0005] In summary, driven by market and technological development, there is an urgent need for a polyacrylonitrile-based carbon fiber with small tow specifications and fine single filament diameter and its preparation process to meet the requirements of many high-precision, ultra-thin, and ultra-fine application scenarios. Summary of the invention
[0006] In view of this, the present invention provides a polyacrylonitrile precursor, a polyacrylonitrile-based carbon fiber and a preparation method thereof, the main purpose of which is to prepare a polyacrylonitrile precursor with small tow specifications and fine single filament diameter, so as to prepare a polyacrylonitrile-based carbon fiber with small tow specifications and fine single filament diameter.
[0007] In order to achieve the above object, the present invention mainly provides the following technical solutions:
[0008] On the one hand, an embodiment of the present invention provides a method for preparing polyacrylonitrile precursor, wherein the method for preparing polyacrylonitrile precursor comprises the following steps:
[0009] The step of preparing polyacrylonitrile spinning solution is as follows: subjecting the reaction monomers to solution polymerization reaction to obtain polyacrylonitrile spinning solution; wherein the reaction monomers include acrylonitrile monomers and comonomers; wherein the mass fraction of the comonomers in the reaction monomers is 5-15wt%;
[0010] Wet spinning step: subjecting the polyacrylonitrile spinning solution to a spinning process, a coagulation forming process, a water washing process, a hot water drawing process, an oiling process, and a drying and densification process in sequence to obtain polyacrylonitrile precursor fibers;
[0011] Among them, during the spinning process, the spinneret used must meet the following conditions: the pore diameter of the spinneret is 20-45μm, and the number of spinneret holes on the spinneret ensures that the K number of the polyacrylonitrile precursor is 0.02-0.5K; preferably, the spacing between the spinneret holes on the spinneret is 5-15 times the pore diameter.
[0012] Preferably, in the step of preparing the polyacrylonitrile spinning solution: the comonomer includes itaconic acid; preferably, the comonomer also includes 2-acrylamide-2-methylpropane sulfonic acid; preferably, in the reaction monomers: the mass ratio of acrylonitrile monomer, itaconic acid, and 2-acrylamide-2-methylpropane sulfonic acid is (85.0-95.0):(5.0-15.0):(0.0-5.0).
[0013] Preferably, in the step of preparing the polyacrylonitrile spinning solution: the reaction solution is subjected to solution polymerization reaction in a reactor to obtain the polyacrylonitrile spinning solution; wherein the reaction solution comprises a reaction monomer, an initiator and a solvent; wherein in the reaction solution, the mass fraction of the reaction monomer is 10-25%; preferably, the initiator is azobisisobutyronitrile; preferably, the amount of the initiator is 0.5-3.0% of the total weight of the reaction monomer; preferably, the solvent is one or more of dimethylformamide, dimethylacetamide, dimethyl sulfoxide, ethylene carbonate, propylene carbonate and γ-butyrolactone; preferably, the polymerization reaction temperature is 30-75°C, and the polymerization reaction time is 10-28h.
[0014] Preferably, in the step of the coagulation molding treatment, the process parameters of the coagulation molding treatment are set as follows: the temperature of the coagulation bath is 45-65°C, the coagulation draw ratio is 0.6-1.25 times, the circulation flow rate of the coagulation bath is 4-14 mm / s, the residence time of the coagulation molding treatment is 0.1-3 min, the mass fraction of the solvent in the coagulation bath is 45-65%, and the mass concentration of the regulator in the coagulation bath is 0.01-0.1 mol / L; preferably, the coagulation bath used for the coagulation molding treatment includes: a solvent, a coagulant, and a regulator; further preferably, the solvent is selected from one or more of dimethylformamide, dimethylacetamide, dimethyl sulfoxide, ethylene carbonate, propylene carbonate, and γ-butyrolactone; the coagulant is deionized water; the regulator is one or more of ethanol, n-propanol, n-butanol, isobutanol, ammonium bicarbonate, and ammonia water; preferably, the coagulation molding treatment adopts a primary coagulation molding treatment.
[0015] Preferably, in the water washing step: the water washing temperature is 50-70°C; the water washing time is 1-3min; preferably, the water washing adopts a primary water washing.
[0016] Preferably, in the step of hot water drawing treatment: the temperature range of the hot water drawing treatment is 70-95°C, and the total drawing ratio is 5-13 times; preferably, the hot water drawing treatment includes a first-level hot water drawing treatment, a second-level hot water drawing treatment, a third-level hot water drawing treatment, a fourth-level hot water drawing treatment, a fifth-level hot water drawing treatment, and a sixth-level hot water drawing treatment; wherein the temperature of the first-level hot water drawing treatment is 70-75°C, and the drawing ratio is 1.1-1.5 times; the second-level hot water drawing treatment is 70-75°C, and the drawing ratio is 1.1-1.5 times; the third-level hot water drawing treatment is 70-75°C, and the drawing ratio is 1.1-1.5 times; the fourth-level hot water drawing treatment is 70-75°C, and the drawing ratio is 1.1-1.5 times; the fifth ... The temperature of the first-level hot water stretching treatment is 75-80℃, and the stretching multiple is 1.3-1.5 times; the temperature of the third-level hot water stretching treatment is 80-83℃, and the stretching multiple is 1.2-1.3 times; the temperature of the fourth-level hot water stretching treatment is 85-88℃, and the stretching multiple is 1.4-1.6 times; the temperature of the fifth-level hot water stretching treatment is 89-91℃, and the stretching multiple is 1.5-1.7 times; the temperature of the sixth-level hot water stretching treatment is 92-95℃, and the stretching multiple is 1.5-1.7 times.
[0017] Preferably, in the oiling step, the concentration of the oil is 0.5-3% (Brix, measured by a refractometer); and / or in the drying and densification step: the number of temperature zones is 5-8, and the temperature of the latter temperature zone in any two adjacent temperature zones is 0-12°C higher than the temperature of the former temperature zone; wherein the temperature of the first temperature zone is 80-100°C; the temperature of the last temperature zone is 115-140°C; and the drying and densification treatment time of each temperature zone is 4-7s.
[0018] On the other hand, an embodiment of the present invention provides a polyacrylonitrile precursor, wherein the single filament diameter of the polyacrylonitrile precursor is 2.9-9 μm, the tensile strength is 850-1450 MPa, the tensile modulus is 9-18 Gpa, and the K number is 0.02-0.5K; preferably, the polyacrylonitrile precursor is prepared by the preparation method of the polyacrylonitrile precursor described in any one of the above items.
[0019] In another aspect, an embodiment of the present invention provides a method for preparing polyacrylonitrile-based carbon fiber, wherein the method for preparing the polyacrylonitrile-based carbon fiber comprises the following steps:
[0020] The polyacrylonitrile precursor is subjected to pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment to obtain polyacrylonitrile-based carbon fibers; wherein the polyacrylonitrile precursor is prepared by the preparation method of the polyacrylonitrile precursor described in any one of the above items;
[0021] Preferably, in the step of preoxidation treatment, the preoxidation treatment time is 15-28 minutes, and the total draft ratio of the preoxidation treatment is 0.8-1.4 times; further preferably, a four-stage hot air medium preoxidation treatment process is adopted; wherein the temperature of the preoxidation treatment is gradually increased, the temperature of the first stage preoxidation treatment is 170-200°C; the temperature of the last stage preoxidation treatment is 240-280°C, and the temperature difference between two adjacent stages of preoxidation treatment is 5-35°C;
[0022] Preferably, in the step of low-temperature carbonization treatment, the temperature of low-temperature carbonization treatment is 300-900° C.; the time of low-temperature carbonization treatment is 1-6 minutes;
[0023] Preferably, in the step of high temperature carbonization treatment, three-stage high temperature carbonization treatment is adopted under a protective atmosphere; preferably, the temperature of the first stage high temperature carbonization treatment is 900-1000°C, the temperature of the last stage high temperature carbonization treatment is 1300-1600°C, and the temperature difference between two adjacent stages of high temperature carbonization treatment is 50-250°C;
[0024] Preferably, the high temperature carbonization treatment time is 0.4-5 min.
[0025] On the other hand, an embodiment of the present invention provides a polyacrylonitrile-based carbon fiber, wherein the K number of the polyacrylonitrile-based carbon fiber is 0.02-0.5K, the single fiber diameter is 1-4.5 μm, the tensile strength is 3.5-4.6 Gpa, and the tensile modulus is 285-330 Gpa; preferably, the roundness of the polyacrylonitrile-based carbon fiber is 0.35-0.95; preferably, the polyacrylonitrile-based carbon fiber is prepared by the above-mentioned preparation method of the polyacrylonitrile-based carbon fiber.
[0026] Compared with the prior art, the polyacrylonitrile precursor, polyacrylonitrile-based carbon fiber and the preparation method thereof of the present invention have at least the following beneficial effects:
[0027] The embodiment of the present invention provides a method for preparing polyacrylonitrile precursor and polyacrylonitrile-based carbon fiber. On the one hand, in the step of preparing polyacrylonitrile spinning solution, the mass fraction of the comonomer in the reaction monomer is 5-15wt%; on the other hand, during the spinning process, the spinneret used must meet the following conditions: the pore size of the spinneret hole is 20-45μm, and the number of spinneret holes on the spinneret ensures that the K number of the polyacrylonitrile precursor is 0.02-0.5K; preferably, the spacing between the spinneret holes on the spinneret is 5-15 times the pore size. It should be noted about the above scheme that: (1) Since it is necessary to prepare carbon fiber with small bundle specifications and fine single filament diameter, the draft multiple of the entire preparation process needs to be significantly increased accordingly. In this case, the fiber filaments are very likely to produce single filament hair. The present invention adopts a polymerization formula with a higher content of comonomer, which is conducive to reducing the rigidity of the polymer molecular chain and improving the flexibility of the polymer chain, thereby improving the spinnability of the polymer, improving the pulling resistance of the entire line of fibers, and reducing hairy fibers; (2) Since the spinnability of the polymer solution is significantly improved, it is conducive to selecting a spinneret with a smaller pore size and a larger pore spacing. In summary, the above scheme of the present invention can realize the preparation of polyacrylonitrile precursor and polyacrylonitrile-based carbon fiber with small tow specifications and fine single filament diameter.
[0028] Furthermore, the embodiment of the present invention provides a method for preparing polyacrylonitrile precursor and polyacrylonitrile-based carbon fiber. Due to the small specifications of the tow and the fine diameter of the single filament, the diameter of the single filament is significantly reduced at all places in the whole preparation process, which is beneficial to: ① coagulation double diffusion process (reduced diffusion path); ② hot drawing and drying densification mass transfer and heat transfer process; ③ pre-oxidation double diffusion process; ④ low-temperature carbonization and high-temperature carbonization reaction material discharge. Therefore, the present invention only needs to use a first-level coagulation bath, a first-level water washing, a six-level hot water drawing, a first-level oiling, a first-level drying densification (less low-temperature zone setting), and no steam drawing and relaxation heat setting process are required. Therefore, the wet spinning process of the present invention is greatly simplified. In addition, due to the increase in the content of the comonomer, the spinnability of the tow is enhanced, the polyacrylonitrile fiber is subjected to multi-stage hot water drawing, the tow diameter is finer, and the pre-oxidation treatment time is greatly shortened. Therefore, compared with the prior art, the preparation process of the present invention is simpler and more efficient.
[0029] Furthermore, in order to realize the preparation of small-sized tows, precursors and carbon fibers with smaller filament diameters: the present invention greatly adjusts the polymerization formula and the whole-line process, significantly increases the content of comonomers (equivalent to an increase in impurities), and simplifies the whole-line process - theoretically, the performance of the fiber is difficult to guarantee. However, due to the small tow, the diameter of the filament is significantly reduced throughout the entire preparation line, which is conducive to ensuring the performance of carbon fibers (tensile strength, tensile modulus) by improving the homogeneity of the fiber filament cross section (the uniformity of the structure of the fiber filament cross section from the inside to the outside). The following scheme is specifically adopted to improve the homogeneity of the fiber: First, a finer spinneret diameter and a larger hole spacing (facilitating double diffusion) are used to ensure the homogeneity of the coagulated filaments. Preferably, the homogeneity of the coagulated filaments is further ensured by setting the process parameters of the first-stage coagulation bath. Furthermore, multi-stage hot water drawing is used to ensure the orientation degree of the polyacrylonitrile precursor. Further, the homogeneity of the pre-oxidized filaments is ensured by a pre-oxidation process. In summary, the present invention can prepare polyacrylonitrile precursor and polyacrylonitrile-based carbon fiber with small tow specifications, fine single filament diameter, excellent tensile modulus and tensile strength.
[0030] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail as follows. DETAILED DESCRIPTION
[0031] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention application are described in detail below in combination with the preferred embodiments. In the following description, different "one embodiment" or "embodiment" do not necessarily refer to the same embodiment. In addition, specific features, structures, or characteristics in one or more embodiments may be combined in any suitable form.
[0032] The embodiment of the present invention provides a polyacrylonitrile precursor, a polyacrylonitrile-based carbon fiber and a preparation method thereof, the main purpose of which is to prepare a polyacrylonitrile-based carbon fiber with a small tow specification and a fine single filament diameter, so as to meet the urgent demand for special fibers in high-precision, ultra-thin, and ultra-fine applications in current special fields (such as micro-satellites, micro-drones, ultra-thin and ultra-large panels, and high-precision medical equipment). The main scheme of the present invention is as follows:
[0033] On the one hand, an embodiment of the present invention provides a method for preparing polyacrylonitrile precursor, which mainly includes the following steps:
[0034] The step of preparing polyacrylonitrile spinning solution is as follows: subjecting the reaction monomers to solution polymerization reaction to obtain polyacrylonitrile spinning solution; wherein the reaction monomers include acrylonitrile monomers and comonomers; wherein in the reaction monomers: the mass fraction of the comonomers is 5-15wt%.
[0035] Specifically, monomer acrylonitrile, comonomer itaconic acid, and comonomer 2-acrylamide-2-methylpropane sulfonic acid are blended in a mass ratio of (85.0-95.0): (5.0-15.0): (0.0-5.0) and added to a reactor with a stirring device; an initiator and a solvent are added to the reactor with a stirring device. The mass percentage of the total monomers in the reaction solution is 10-25%. Azobisisobutylcyanide is used as an initiator, and the amount of the initiator is 0.5-3.0% of the total weight of the monomers. The solvent is selected from one of dimethylformamide, dimethylacetamide, dimethyl sulfoxide, ethylene carbonate, propylene carbonate, and γ-butyrolactone, and solution polymerization is carried out. The polymerization reaction temperature is controlled in the range of 30-75°C, and the polymerization reaction time is 10-28h to obtain a polyacrylonitrile spinning solution.
[0036] The wet spinning step is to sequentially subject the polyacrylonitrile spinning solution to a spinning treatment, a coagulation and forming treatment, a water washing treatment, a hot water drawing treatment, an oiling treatment, and a drying and densification treatment to obtain polyacrylonitrile precursor.
[0037] Among them, during the spinning process, the spinneret used must meet the following conditions: the pore diameter of the spinneret is 20-45μm, and the number of spinneret holes on the spinneret ensures that the K number of the polyacrylonitrile precursor is 0.02-0.5K; preferably, the spacing between the spinneret holes on the spinneret is 5-15 times the pore diameter.
[0038] Among them, the coagulation molding treatment: after the spinning solution is ejected from the spinneret, it is subjected to a primary coagulation bath coagulation molding treatment. Among them, the coagulation bath liquid is composed of three parts: solvent, coagulant, and regulator; the solvent is selected from one or more of dimethylformamide, dimethylacetamide, dimethyl sulfoxide, ethylene carbonate, propylene carbonate, and γ-butyrolactone; the coagulant is deionized water; the regulator is selected from one or more of ethanol, n-propanol, n-butanol, isobutanol, ammonium bicarbonate, and ammonia water.
[0039] The process parameters of the primary coagulation molding treatment are set as follows: the temperature of the coagulation bath is 45-65°C; the coagulation stretching rate is 0.6-1.25 times; the circulation flow rate of the coagulation bath is 4-14mm / s; the residence time of the coagulation molding treatment is 0.1-3min; the mass fraction of the solvent in the coagulation bath is 45-65%; the mass concentration of the regulator in the coagulation bath is 0.01-0.1mol / L.
[0040] Among them, water washing treatment (primary water washing treatment): water washing temperature is 50-70°C; water washing time is 1-3min.
[0041] Among them, hot water drawing treatment: the temperature range of the drawing treatment is 70-95℃, and the total drawing ratio is 5-13 times. Six-level hot water drawing treatment is adopted, specifically, the temperature of the first-level hot water drawing treatment is 70-75℃, and the drawing ratio is 1.1-1.5 times; the temperature of the second-level hot water drawing treatment is 75-80℃, and the drawing ratio is 1.3-1.5 times; the temperature of the third-level hot water drawing treatment is 80-83℃, and the drawing ratio is 1.2-1.3 times; the temperature of the fourth-level hot water drawing treatment is 85-88℃, and the drawing ratio is 1.4-1.6 times; the temperature of the fifth-level hot water drawing treatment is 89-91℃, and the drawing ratio is 1.5-1.7 times; the temperature of the sixth-level hot water drawing treatment is 92-95℃, and the drawing ratio is 1.5-1.7 times.
[0042] Among them, oiling treatment: using silicone oil, the oil concentration is 0.5-3% (Brix).
[0043] Among them, the drying and densification treatment: adopt low temperature and long time gradient drying and densification treatment. The number of temperature zones is 5-8, and the temperature of the latter temperature zone in any two adjacent temperature zones is 0-12℃ higher than that of the former temperature zone; among them, the temperature of the first temperature zone is 80-100℃; the temperature of the last temperature zone is 115-140℃; the drying and densification treatment time of each temperature zone is 4-7s.
[0044] On the other hand, an embodiment of the present invention further provides a polyacrylonitrile precursor, which is prepared by the above-mentioned method for preparing the polyacrylonitrile precursor.
[0045] On the other hand, an embodiment of the present invention further provides a method for preparing polyacrylonitrile-based carbon fiber, comprising the following steps:
[0046] Preoxidation treatment: The polyacrylonitrile precursor prepared above is subjected to preoxidation treatment to obtain preoxidation treated fibers. A four-stage hot air medium preoxidation treatment process is adopted; the temperature of the preoxidation treatment is gradually increased, the temperature of the first stage preoxidation treatment is 170-200°C; the temperature of the last stage preoxidation treatment is 240-280°C, and the temperature difference between two adjacent stages of preoxidation treatment is 5-35°C.
[0047] Low-temperature carbonization treatment: The pre-oxidation treated fiber is subjected to low-temperature carbonization treatment to obtain low-temperature carbonized fiber.
[0048] The low-temperature carbonization treatment is carried out under the protection of high-purity nitrogen, wherein the temperature of the low-temperature carbonization treatment is 300-900° C. and the time of the low-temperature carbonization treatment is 1-6 minutes.
[0049] High temperature carbonization treatment: The fiber after low temperature carbonization treatment is subjected to high temperature carbonization treatment to obtain high temperature carbonized fiber.
[0050] Wherein, high temperature carbonization treatment is carried out under the protection of high purity nitrogen. Wherein, under the protective atmosphere, three-stage high temperature carbonization treatment is adopted; preferably, the temperature of the first stage high temperature carbonization treatment is 900-1000°C, the temperature of the last stage high temperature carbonization treatment is 1300-1600°C, and the temperature difference between the two adjacent stages of high temperature carbonization treatment is 50-250°C; preferably, the time of high temperature carbonization treatment is 0.4-5min.
[0051] On the other hand, an embodiment of the present invention provides a polyacrylonitrile-based carbon fiber, wherein the K number of the polyacrylonitrile-based carbon fiber is 0.02-0.5K, the single fiber diameter is 1-4.5 μm, the tensile strength is 3.5-4.6 Gpa, the tensile modulus is 285-330 Gpa, and the roundness is 0.35-0.95 (the roundness here refers to: the ratio of the short axis to the long axis of the fiber cross section); preferably, the polyacrylonitrile-based carbon fiber is prepared by the above-mentioned method for preparing the polyacrylonitrile-based carbon fiber.
[0052] Here, it is necessary to explain the above scheme:
[0053] 1) The K number of the existing commercial polyacrylonitrile-based carbon fiber is ≥1k, and the diameter of the single fiber is 4.7-7μm. Different from the prior art, the K number of the polyacrylonitrile-based carbon fiber of the present invention is 0.02-0.5K, and the diameter of the single fiber is 1-4.5μm.
[0054] 2) Regarding the polymerization reaction formula: the mass proportion of the comonomer (the second monomer and the third monomer) in the existing polymerization reaction formula in the total monomers is ≤5wt%, and generally preferably ≤3wt%. Different from the prior art, the mass proportion of the comonomer (the second monomer and the third monomer) in the present invention in the total monomers is 5-15wt%.
[0055] It should be noted here that: since it is necessary to prepare carbon fiber with small tow specifications and fine single filament diameter, the drafting multiple of the entire preparation process (spinning, pre-oxidation) needs to be significantly increased accordingly. In this case, the fiber filaments are very likely to produce single filament hairs.
[0056] Here, in order to improve the pulling resistance and spinnability of the entire fiber line: the present invention adopts a polymerization formula with a higher comonomer content, which is beneficial to reduce the rigidity of the polymer molecular chain, improve the flexibility of the polymer chain, improve the spinnability of the polymer, and improve the pulling resistance of the entire fiber line.
[0057] 3) The diameter of the spinneret hole is 20-45 μm, and the number of the spinneret holes on the spinneret plate ensures that the K number of the polyacrylonitrile precursor is 0.02-0.5K; preferably, the spacing between the spinneret holes on the spinneret plate is 5-15 times the diameter of the hole.
[0058] It should be noted here that: due to the significant increase in the comonomer, the spinnability of the polymer solution is significantly improved, which is conducive to the selection of a spinneret with a smaller pore size and a larger pore spacing.
[0059] Wet spinning: The existing wet spinning process uses multi-stage coagulation, multi-stage washing, hot water drawing, oiling, drying densification, steam drawing and relaxation heat setting. Different from the existing wet spinning process, the present invention uses a first-stage coagulation bath, a first-stage washing, six-stage hot water drawing, a first-stage oiling, a first-stage drying densification, and no steam drawing and relaxation heat setting process.
[0060] Pre-oxidation treatment process: The pre-oxidation treatment time of the present invention is short, specifically 15-28 minutes.
[0061] Specifically, due to the small specifications of the filament bundles and the fine diameter of the single filaments (compared with existing carbon fibers), the diameter of the single filaments at all points in the entire preparation process is significantly reduced, which is beneficial to: ① solidification double diffusion process (reduced diffusion path); ② hot drawing and drying densification mass transfer and heat transfer process; ③ pre-oxidation double diffusion process; ④ low-temperature carbonization and high-temperature carbonization reaction material discharge.
[0062] Therefore, the present invention only needs to adopt one-stage coagulation bath, one-stage water washing, six-stage hot water drawing, one-stage oiling, one-stage drying densification, and no steam drawing and relaxation heat setting process is required; in addition, a shorter pre-oxidation treatment time of 15-28 minutes is adopted.
[0063] Since the single-bundle yarn has a small specification (0.02-0.5k) and a thin single-filament diameter, mass transfer, heat transfer, and fiber orientation improvement during fiber coagulation, water washing, and hot drawing are relatively easy, and therefore, the wet spinning process of the present invention is greatly simplified.
[0064] In addition, with the increase of comonomer content, the spinnability of the tow is enhanced, the polyacrylonitrile fiber is subjected to multi-stage hot water drawing, the tow diameter is finer, and the pre-oxidation treatment time is greatly shortened (the pre-oxidation treatment time for traditional commercial carbon fiber preparation is 30-75 minutes).
[0065] Compared with the prior art, the preparation process of the present invention is simpler and more efficient.
[0066] 4) In order to achieve small-size tows and smaller single-filament diameters: The present invention greatly adjusts the polymerization formula and the entire process, significantly increases the content of comonomers (equivalent to an increase in impurities), and simplifies the entire process - in theory, the fiber performance is difficult to guarantee. However, due to the small tow, the single-filament diameter is significantly reduced throughout the entire preparation line, which is conducive to ensuring the performance of carbon fibers (tensile strength, tensile modulus) by improving the homogeneity of the fiber single-filament cross section (the uniformity of the structure of the fiber single-filament cross section from the inside to the outside), as follows:
[0067] First, a finer spinneret diameter and a larger hole spacing (facilitating double diffusion) are used to ensure the homogenization of the coagulated filaments. Preferably, the homogenization of the coagulated filaments is further ensured by setting the process parameters of the primary coagulation bath. Furthermore, multi-stage hot water drawing is used to ensure the orientation of the polyacrylonitrile precursor. Further, the homogenization of the pre-oxidized filaments is ensured by a pre-oxidation process.
[0068] The present invention is further described below by specific embodiments:
[0069] Example 1
[0070] In this embodiment, a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber with a tow specification of 0.02K are prepared, and the main preparation steps are as follows:
[0071] The solvent of the coagulation bath is dimethyl sulfoxide, the coagulant is deionized water, and the regulator is ammonia water.
[0072] The process parameters of the primary coagulation molding are as follows: the temperature of the coagulation bath is 60°C; the coagulation draft ratio is 1.2 times; the circulation flow rate of the coagulation bath is 10 mm / s; the residence time of the coagulation molding treatment is 1 min; the mass fraction of the solvent in the coagulation bath is 65%; the mass concentration of the regulator in the coagulation bath is 0.1 mol / L) Steps for preparing the polyacrylonitrile spinning solution:
[0073] The monomers of acrylonitrile, itaconic acid and 2-acrylamido-2-methylpropane sulfonic acid are blended in a mass ratio of 85.5:14.5:0 and added to a reactor with a stirring device; and an initiator and a solvent are added to the reactor to carry out a solution polymerization reaction. Among them, the total mass of the monomers accounts for 19.5wt% of the mass percentage of the reaction solution. Azobisisobutyl cyanide is used as an initiator, and the amount of the initiator is 1.5wt% of the total weight of the monomers. The solvent is dimethyl sulfoxide. Among them, the polymerization reaction temperature is 65°C, and the polymerization reaction time is 17h to obtain a polyacrylonitrile spinning solution.
[0074] 2) Spinning and solidification molding (primary solidification molding)
[0075] Wet spinning is adopted, the diameter of the spinneret holes on the spinneret plate is 20 μm, and the number of the spinneret holes on the spinneret plate ensures that the K number of the polyacrylonitrile precursor is 0.02K; preferably, the spacing between the spinneret holes on the spinneret plate is 15 times the diameter of the hole.
[0076] After the spinning solution is ejected from the spinneret, it is coagulated in a primary coagulation bath.
[0077] 3) Water washing process (primary water washing process)
[0078] The temperature of the water washing treatment is 60°C, and the time of the water washing treatment is 2 minutes.
[0079] 4) Six-stage hot water drawing process
[0080] The temperature of the first-stage hot water drawing treatment is 75°C, and the drawing ratio is 1.5 times;
[0081] The temperature of the second-stage hot water drawing treatment is 80°C, and the drawing ratio is 1.5 times;
[0082] The temperature of the third-stage hot water drawing treatment is 83°C, and the drawing ratio is 1.3 times;
[0083] The temperature of the fourth-level hot water drawing treatment is 88°C, and the drawing ratio is 1.6 times;
[0084] The temperature of the five-stage hot water drawing treatment is 91°C, and the drawing ratio is 1.7 times;
[0085] The temperature of the six-stage hot water drawing treatment is 95°C, and the drawing ratio is 1.7 times.
[0086] 5) Oiling process
[0087] Use self-prepared silicone oil, the concentration of the oil is 0.8%.
[0088] 6) Drying and densification process
[0089] There are 5 temperature zone gradient levels; the temperature zone gradients are: 95°C, 100°C, 108°C, 115°C, 118°C; the time for each drying and densification treatment is 4s.
[0090] After drying and densification, polyacrylonitrile precursor was obtained. The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this example are shown in Table 1.
[0091] The polyacrylonitrile precursor is subjected to pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment in sequence to obtain polypropylene-based carbon fibers, as follows:
[0092] 7) Pre-oxidation treatment process
[0093] Under hot air medium, a 4-stage pre-oxidation process is adopted. The pre-oxidation treatment temperatures are: 198℃, 210℃, 230℃, 253℃; the total drafting multiple of the pre-oxidation treatment is 1.4 times; the total residence time of the pre-oxidation treatment is 15min.
[0094] 8) Low temperature carbonization process
[0095] Under the protection of high-purity nitrogen, the temperature of the low-temperature carbonization treatment is 300-900°C; the time of the low-temperature carbonization treatment is 4 minutes.
[0096] 9) High temperature carbonization process
[0097] Under the protection of high-purity nitrogen, a three-stage high-temperature carbonization treatment was adopted; the high-temperature carbonization temperatures were 950°C, 1200°C, and 1450°C, respectively; and the high-temperature carbonization treatment time was 2 minutes.
[0098] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fibers prepared in this example are shown in Table 2.
[0099] Example 2
[0100] In this embodiment, a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber with a tow specification of 0.02K are prepared, and the main preparation steps are as follows:
[0101] 1) Preparation of polyacrylonitrile spinning solution steps:
[0102] The monomers acrylonitrile, itaconic acid and 2-acrylamido-2-methylpropane sulfonic acid are blended in a mass ratio of 90:9:1 and added to a reactor with a stirring device; and an initiator and a solvent are added to the reactor to carry out a solution polymerization reaction. The total mass of the monomers accounts for 21wt% of the mass percentage of the reaction solution. Azobisisobutyl cyanide is used as an initiator, and the amount of the initiator is 2wt% of the total weight of the monomers. The solvent is dimethyl sulfoxide. The polymerization reaction temperature is 66°C, and the polymerization reaction time is 15h to obtain a polyacrylonitrile spinning solution.
[0103] 2) Spinning and solidification molding (primary solidification molding)
[0104] Wet spinning is adopted, the diameter of the spinneret holes on the spinneret plate is 30 μm, and the number of the spinneret holes on the spinneret plate ensures that the K number of the polyacrylonitrile precursor is 0.02K; preferably, the spacing between the spinneret holes on the spinneret plate is 10 times the diameter of the hole.
[0105] After the spinning solution is ejected from the spinneret, it is solidified and formed in a primary coagulation bath, wherein the solvent of the coagulation bath is dimethyl sulfoxide, the coagulant is deionized water, and the regulator is ammonia water.
[0106] The process parameters of primary solidification molding are as follows: the temperature of the solidification bath is 50°C; the solidification drawing ratio is 0.9 times; the circulation flow rate of the solidification bath is 10 mm / s; the residence time of the solidification molding treatment is 1 min; the mass fraction of the solvent in the solidification bath is 55%; the mass concentration of the regulator in the solidification bath is 0.02 mol / L.
[0107] 3) Water washing process (primary water washing process)
[0108] The temperature of the water washing treatment is 50°C, and the time of the water washing treatment is 3 minutes.
[0109] 4) Six-stage hot water drawing process
[0110] The temperature of the first-stage hot water drawing treatment is 72°C, and the drawing ratio is 1.3 times;
[0111] The temperature of the second-stage hot water drawing treatment is 78°C, and the drawing ratio is 1.4 times;
[0112] The temperature of the third-stage hot water drawing treatment is 82°C, and the drawing ratio is 1.25 times;
[0113] The temperature of the fourth-level hot water drawing treatment is 86°C, and the drawing ratio is 1.5 times;
[0114] The temperature of the five-stage hot water drawing treatment is 90°C, and the drawing ratio is 1.6 times;
[0115] The temperature of the sixth-level hot water drawing treatment is 94°C, and the drawing ratio is 1.6 times.
[0116] 5) Oiling process
[0117] Use self-prepared silicone oil, the oil concentration is 1.5%.
[0118] 6) Drying and densification process
[0119] There are 7 temperature zone gradient levels; the temperature zone gradients are: 95°C, 100°C, 108°C, 110°C, 115°C, 118°C, 125°C; the time for each level of drying and densification treatment is 6s.
[0120] After drying and densification, polyacrylonitrile precursor was obtained. The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this example are shown in Table 1.
[0121] The polyacrylonitrile precursor is subjected to pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment in sequence to obtain polypropylene-based carbon fibers, as follows:
[0122] 7) Pre-oxidation treatment process
[0123] Under hot air medium, a 4-stage pre-oxidation process is adopted. The pre-oxidation treatment temperatures are: 195℃, 210℃, 235℃, 255℃; the total drafting multiple of the pre-oxidation treatment is 1 times; the total residence time of the pre-oxidation treatment is 22min.
[0124] 8) Low temperature carbonization process
[0125] Under the protection of high-purity nitrogen, the temperature of the low-temperature carbonization treatment is 300-900°C; the time of the low-temperature carbonization treatment is 4 minutes.
[0126] 9) High temperature carbonization process
[0127] Under the protection of high-purity nitrogen, a three-stage high-temperature carbonization treatment was adopted; the high-temperature carbonization temperatures were 1000°C, 1250°C, and 1500°C, respectively; and the high-temperature carbonization treatment time was 2 minutes.
[0128] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fibers prepared in this example are shown in Table 2.
[0129] Example 3
[0130] In this embodiment, a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber with a tow specification of 0.02K are prepared, and the main preparation steps are as follows:
[0131] 1) Preparation of polyacrylonitrile spinning solution steps:
[0132] The monomers acrylonitrile, itaconic acid and 2-acrylamido-2-methylpropane sulfonic acid are blended in a mass ratio of 94.9:5:0.1 and added to a reactor with a stirring device; and an initiator and a solvent are added to the reactor to carry out a solution polymerization reaction. The total mass of the monomers accounts for 21wt% of the mass percentage of the reaction solution. Azobisisobutyl cyanide is used as an initiator, and the amount of the initiator is 2wt% of the total weight of the monomers. The solvent is dimethyl sulfoxide. The polymerization reaction temperature is 68°C, and the polymerization reaction time is 15h to obtain a polyacrylonitrile spinning solution.
[0133] 2) Spinning and solidification molding (primary solidification molding)
[0134] Wet spinning is adopted, the diameter of the spinneret holes on the spinneret plate is 45 μm, and the number of the spinneret holes on the spinneret plate ensures that the K number of the polyacrylonitrile precursor is 0.02K; preferably, the spacing between the spinneret holes on the spinneret plate is 5 times the diameter of the hole.
[0135] After the spinning solution is ejected from the spinneret, it is solidified and formed in a primary coagulation bath, wherein the solvent of the coagulation bath is dimethyl sulfoxide, the coagulant is deionized water, and the regulator is ammonia water.
[0136] The process parameters of primary coagulation molding are as follows: the temperature of the coagulation bath is 45°C; the coagulation drawing ratio is 0.65 times; the circulation flow rate of the coagulation bath is 10 mm / s; the residence time of the coagulation molding treatment is 1 min; the mass fraction of the solvent in the coagulation bath is 48%; the mass concentration of the regulator in the coagulation bath is 0.01 mol / L.
[0137] 3) Water washing process (primary water washing process)
[0138] The temperature of the water washing treatment is 70°C, and the time of the water washing treatment is 1 min.
[0139] 4) Six-stage hot water drawing process
[0140] The temperature of the first-stage hot water drawing treatment is 70°C, and the drawing ratio is 1.1 times;
[0141] The temperature of the second-stage hot water drawing treatment is 75°C, and the drawing ratio is 1.3 times;
[0142] The temperature of the third-stage hot water drawing treatment is 80°C, and the drawing ratio is 1.2 times;
[0143] The temperature of the fourth-level hot water drawing treatment is 85°C, and the drawing ratio is 1.4 times;
[0144] The temperature of the five-stage hot water drawing treatment is 89°C, and the drawing ratio is 1.5 times;
[0145] The temperature of the sixth-level hot water drawing treatment is 92°C, and the drawing multiple is 1.5 times.
[0146] 5) Oiling process
[0147] Use self-prepared silicone oil, the concentration of the oil is 3%.
[0148] 6) Drying and densification process
[0149] There are 8 temperature zone gradient levels; the temperature zone gradients are: 90℃, 95℃, 100℃, 105℃, 108℃, 115℃, 125℃, 135℃; the time for each level of drying and densification treatment is 7s.
[0150] After drying and densification, polyacrylonitrile precursor was obtained. The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this example are shown in Table 1.
[0151] The polyacrylonitrile precursor is subjected to pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment in sequence to obtain polypropylene-based carbon fibers, as follows:
[0152] 7) Pre-oxidation treatment process
[0153] Under hot air medium, a 4-stage pre-oxidation process is adopted. The pre-oxidation treatment temperatures are: 200℃, 210℃, 245℃, 265℃; the total drafting multiple of the pre-oxidation treatment is 0.8 times; the total residence time of the pre-oxidation treatment is 28min.
[0154] 8) Low temperature carbonization process
[0155] Under the protection of high-purity nitrogen, the temperature of the low-temperature carbonization treatment is 300-900°C; the time of the low-temperature carbonization treatment is 4 minutes.
[0156] 9) High temperature carbonization process
[0157] Under the protection of high-purity nitrogen, a three-stage high-temperature carbonization treatment was adopted; the carbonization temperatures were 900°C, 1150°C, and 1400°C, respectively; and the high-temperature carbonization treatment time was 2 minutes.
[0158] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fibers prepared in this example are shown in Table 2.
[0159] Example 4
[0160] This embodiment prepares a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber, which is different from the embodiment 1 in that the tow specification is different, and the tow specification of this embodiment is 0.1K. Other steps and process parameters are the same as those of the embodiment 1.
[0161] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this example are shown in Table 1.
[0162] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fibers prepared in this example are shown in Table 2.
[0163] Example 5
[0164] This embodiment prepares a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber, which is different from the embodiment 2 in that the tow specification is different, and the tow specification of this embodiment is 0.1K. Other steps and process parameters are the same as those of the embodiment 2.
[0165] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this example are shown in Table 1.
[0166] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fibers prepared in this example are shown in Table 2.
[0167] Example 6
[0168] This embodiment prepares a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber, which is different from the embodiment 3 in that the tow specification is different, and the tow specification of this embodiment is 0.1K. Other steps and process parameters are the same as those of the embodiment 3.
[0169] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this example are shown in Table 1.
[0170] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fibers prepared in this example are shown in Table 2.
[0171] Example 7
[0172] This embodiment prepares a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber, which is different from the embodiment 1 in that the tow specification is different, and the tow specification of this embodiment is 0.5K. Other steps and process parameters are the same as those of the embodiment 1.
[0173] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this example are shown in Table 1.
[0174] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fibers prepared in this example are shown in Table 2.
[0175] Example 8
[0176] This embodiment prepares a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber, which is different from the embodiment 2 in that the tow specification is different, and the tow specification of this embodiment is 0.5K. Other steps and process parameters are the same as those of the embodiment 2.
[0177] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this example are shown in Table 1.
[0178] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fibers prepared in this example are shown in Table 2.
[0179] Example 9
[0180] This embodiment prepares a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber, which is different from the embodiment 3 in that the tow specification is different, and the tow specification of this embodiment is 0.5K. Other steps and process parameters are the same as those of the embodiment 3.
[0181] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this example are shown in Table 1.
[0182] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fibers prepared in this example are shown in Table 2.
[0183] Comparative Example 1
[0184] This comparative example prepares a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber, which is different from Example 1 in that the monomer acrylonitrile, the monomer itaconic acid, and the 2-acrylamide-2-methylpropane sulfonic acid are mixed in a mass ratio of 98:2:0. The other steps and process parameters are the same as those in Example 1.
[0185] In the spinning process of this comparative example, the polymer solution has poor spinnability, and filaments and broken filaments are easily produced during the spinning, coagulation, washing, hot drawing and drying processes, and it is difficult to complete the filament collection.
[0186] This comparative example cannot complete the production of finished products and qualified raw silk, and cannot complete the subsequent carbon fiber preparation.
[0187] Comparative Example 2
[0188] This comparative example prepares a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber, which is different from Example 1 in that the tow specification is different, and the tow specification of this example is 1K. Other steps and process parameters are the same as those of Example 1.
[0189] The tow specification is 1k. The larger the tow specification, the less favorable the mass and heat transfer. The drying densification residence time and the pre-oxidation residence time are insufficient, resulting in a decrease in the uniformity of the radial structure of the fiber. The final performance of the carbon fiber is inferior to that of Example 1.
[0190] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this comparative example are shown in Table 1.
[0191] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fiber prepared in this comparative example are shown in Table 2.
[0192] Comparative Example 3
[0193] This comparative example prepares a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber, which is different from Example 1 in that the temperature of the coagulation bath is 70°C, the coagulation draft ratio is 0.55 times, and the mass fraction of the solvent in the coagulation bath is 40%. Other steps and process parameters are the same as those in Example 1.
[0194] The coagulation molding process conditions in this comparative example are not matched reasonably, resulting in reduced uniformity of the radial structure of the fiber, and the performance of the final carbon fiber is not as good as that of Example 1.
[0195] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this comparative example are shown in Table 1.
[0196] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fiber prepared in this comparative example are shown in Table 2.
[0197] Comparative Example 4
[0198] This comparative example prepares a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber, which is different from Example 1 in that the total residence time of the pre-oxidation treatment is 12 minutes. The other steps and process parameters are the same as those of Example 1.
[0199] The pre-oxidation residence time in this comparative example is insufficient, resulting in reduced uniformity of the radial structure of the fiber, and the performance of the final carbon fiber is inferior to that of Example 1.
[0200] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this comparative example are shown in Table 1.
[0201] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fiber prepared in this comparative example are shown in Table 2.
[0202] Comparative Example 5
[0203] This comparative example prepares a polyacrylonitrile precursor and a polyacrylonitrile-based carbon fiber, which is different from Example 1 in that: the first-level hot water drawing multiple is 1.9 times; the second-level hot water drawing multiple is 1.8 times; the third-level hot water drawing multiple is 1.6 times; the fourth-level hot water drawing multiple is 1.3 times; the fifth-level hot water drawing multiple is 1.3 times; and the sixth-level hot water drawing multiple is 1.4 times. Other steps and process parameters are the same as those in Example 1.
[0204] The hot water drawing multiple parameter matching is unreasonable (high at the front and low at the back), resulting in insufficient orientation of the polyacrylonitrile fiber, and the performance of the final carbon fiber is not as good as that of Example 1.
[0205] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based precursor prepared in this comparative example are shown in Table 1.
[0206] The properties (K number, single filament diameter, roundness) and performance (tensile strength, tensile modulus) of the polyacrylonitrile-based carbon fiber prepared in this comparative example are shown in Table 2.
[0207] Table 1 shows the tow specifications, properties and mechanical properties of the polyacrylonitrile-based precursor fibers prepared in Examples 1-9 and Comparative Examples 1-5.
[0208] Table 1
[0209]
[0210] Table 2 shows the tow specifications, properties and mechanical properties of the polyacrylonitrile-based carbon fibers prepared in Examples 1-9 and Comparative Examples 1-5.
[0211] Table 2
[0212]
[0213] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing polyacrylonitrile precursor, characterized in that: The preparation method of the polyacrylonitrile precursor comprises the following steps: The step of preparing polyacrylonitrile spinning solution is as follows: subjecting the reaction monomers to solution polymerization reaction to obtain polyacrylonitrile spinning solution; wherein the reaction monomers include acrylonitrile monomers and comonomers; wherein the mass fraction of the comonomers in the reaction monomers is 5-15wt%; Wet spinning step: subjecting the polyacrylonitrile spinning solution to a spinning process, a coagulation forming process, a water washing process, a hot water drawing process, an oiling process, and a drying and densification process in sequence to obtain polyacrylonitrile precursor fibers; Among them, during the spinning process, the spinneret used must meet the following conditions: the pore diameter of the spinneret is 20-45μm, and the number of spinneret holes on the spinneret ensures that the K number of the polyacrylonitrile precursor is 0.02-0.5K; preferably, the spacing between the spinneret holes on the spinneret is 5-15 times the pore diameter.
2. The method for preparing polyacrylonitrile precursor according to claim 1, characterized in that: In the step of preparing polyacrylonitrile spinning solution: The comonomer includes itaconic acid; Preferably, the comonomer further comprises 2-acrylamido-2-methylpropane sulfonic acid; Preferably, in the reaction monomers, the mass ratio of acrylonitrile monomer, itaconic acid, and 2-acrylamide-2-methylpropane sulfonic acid is (85.0-95.0):(5.0-15.0):(0.0-5.0).
3. The method for preparing polyacrylonitrile precursor according to claim 1 or 2, characterized in that: In the step of preparing the polyacrylonitrile spinning solution: The reaction solution is subjected to a solution polymerization reaction in a reactor to obtain a polyacrylonitrile spinning solution; wherein the reaction solution comprises a reaction monomer, an initiator, and a solvent; wherein the mass fraction of the reaction monomer in the reaction solution is 10-25%; Preferably, the initiator is azobisisobutyronitrile; Preferably, the amount of the initiator is 0.5-3.0% of the total weight of the reaction monomers; Preferably, the solvent is selected from one or more of dimethylformamide, dimethylacetamide, dimethyl sulfoxide, ethylene carbonate, propylene carbonate, and γ-butyrolactone; Preferably, the polymerization temperature is 30-75° C., and the polymerization time is 10-28 h.
4. The method for preparing polyacrylonitrile precursor according to any one of claims 1 to 3, characterized in that: In the step of the solidification molding process: The process parameters of the coagulation molding treatment are set as follows: the temperature of the coagulation bath is 45-65°C, the coagulation draft ratio is 0.6-1.25 times, the circulation flow rate of the coagulation bath is 4-14 mm / s, the residence time of the coagulation molding treatment is 0.1-3 min, the mass fraction of the solvent in the coagulation bath is 45-65%, and the mass concentration of the regulator in the coagulation bath is 0.01-0.1 mol / L; Preferably, the coagulation bath used for the coagulation molding treatment comprises: a solvent, a coagulant, and a regulator; further preferably, the solvent is selected from one or more of dimethylformamide, dimethylacetamide, dimethyl sulfoxide, ethylene carbonate, propylene carbonate, and γ-butyrolactone; the coagulant is deionized water; the regulator is selected from one or more of ethanol, n-propanol, n-butanol, isobutanol, ammonium bicarbonate, and ammonia water; Preferably, the solidification molding process adopts a primary solidification molding process.
5. The method for preparing polyacrylonitrile precursor according to any one of claims 1 to 4, characterized in that: In the step of the water washing treatment: The water washing treatment temperature is 50-70°C; the water washing treatment time is 1-3min; Preferably, the water washing treatment adopts a primary water washing treatment.
6. The method for preparing polyacrylonitrile precursor according to any one of claims 1 to 5, characterized in that: In the step of hot water drawing treatment: The temperature range of the hot water drawing treatment is 70-95°C, and the total drawing ratio is 5-13 times; Preferably, the hot water stretching treatment includes a first-level hot water stretching treatment, a second-level hot water stretching treatment, a third-level hot water stretching treatment, a fourth-level hot water stretching treatment, a fifth-level hot water stretching treatment, and a sixth-level hot water stretching treatment; wherein, the temperature of the first-level hot water stretching treatment is 70-75°C, and the stretching multiple is 1.1-1.5 times; the temperature of the second-level hot water stretching treatment is 75-80°C, and the stretching multiple is 1.3-1.5 times; the temperature of the third-level hot water stretching treatment is 80-83°C, and the stretching multiple is 1.2-1.3 times; the temperature of the fourth-level hot water stretching treatment is 85-88°C, and the stretching multiple is 1.4-1.6 times; the temperature of the fifth-level hot water stretching treatment is 89-91°C, and the stretching multiple is 1.5-1.7 times; the temperature of the sixth-level hot water stretching treatment is 92-95°C, and the stretching multiple is 1.5-1.7 times.
7. The method for preparing polyacrylonitrile precursor according to any one of claims 1 to 6, characterized in that: In the oiling step, the concentration of the oil is 0.5-3%; and / or In the drying and densification treatment step: the number of temperature zones is 5-8, and the temperature of the latter temperature zone in any two adjacent temperature zones is 0-12°C higher than that of the former temperature zone; wherein the temperature of the first temperature zone is 80-100°C; the temperature of the last temperature zone is 115-140°C; and the drying and densification treatment time of each temperature zone is 4-7s.
8. A polyacrylonitrile precursor, characterized in that: The single filament diameter of the polyacrylonitrile precursor is 2.9-9 μm, the tensile strength is 850-1450 MPa, the tensile modulus is 9-18 Gpa, and the K number is 0.02-0.5K; preferably, the polyacrylonitrile precursor is prepared by the preparation method of the polyacrylonitrile precursor according to any one of claims 1-7.
9. A method for preparing polyacrylonitrile-based carbon fiber, characterized in that: The method for preparing the polyacrylonitrile-based carbon fiber comprises the following steps: The polyacrylonitrile precursor is subjected to pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment to obtain polyacrylonitrile-based carbon fibers; Wherein, the polyacrylonitrile precursor is prepared by the preparation method of the polyacrylonitrile precursor according to any one of claims 1 to 7; Preferably, in the step of pre-oxidation treatment, the pre-oxidation treatment time is 15-28 minutes, and the total draft ratio of the pre-oxidation treatment is 0.8-1.4 times; Further preferably, a four-stage hot air medium preoxidation treatment process is adopted; wherein the temperature of the preoxidation treatment is gradually increased, the temperature of the first stage preoxidation treatment is 170-200°C; the temperature of the last stage preoxidation treatment is 240-280°C, and the temperature difference between two adjacent stages of preoxidation treatment is 5-35°C; Preferably, in the step of low-temperature carbonization treatment, the temperature of low-temperature carbonization treatment is 300-900° C.; the time of low-temperature carbonization treatment is 1-6 minutes; Preferably, in the step of high temperature carbonization treatment, three-stage high temperature carbonization treatment is adopted under a protective atmosphere; preferably, the temperature of the first stage high temperature carbonization treatment is 900-1000°C, the temperature of the last stage high temperature carbonization treatment is 1300-1600°C, and the temperature difference between two adjacent stages of high temperature carbonization treatment is 50-250°C; Preferably, the high temperature carbonization treatment time is 0.4-5 min.
10. A polyacrylonitrile-based carbon fiber, characterized in that: The polyacrylonitrile-based carbon fiber has a K number of 0.02-0.5K, a single filament diameter of 1-4.5 μm, a tensile strength of 3.5-4.6 Gpa, and a tensile modulus of 285-330 Gpa; Preferably, the roundness of the polyacrylonitrile-based carbon fiber is 0.35-0.95; Preferably, the polyacrylonitrile-based carbon fiber is prepared by the preparation method of the polyacrylonitrile-based carbon fiber according to claim 9.