Production method of water-based basketball leather base cloth

By impregnating and modifying nonwoven fabrics with waterborne polyurethane resin emulsion, combined with a drying process, an environmentally friendly waterborne basketball leather base fabric with excellent wear resistance was prepared, solving the problems of environmentally unfriendly production and insufficient wear resistance in existing technologies.

CN118958009APending Publication Date: 2024-11-15WANHUA NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411166358.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The current production process for basketball leather base fabric is not environmentally friendly and has poor abrasion resistance.

Method used

Nonwoven fabric was impregnated with waterborne polyurethane resin emulsion, and waterborne basketball leather base fabric was prepared by modification and foaming treatment combined with drying process. Modified waterborne polyurethane resin emulsion, crosslinking agent and nanoparticles were used to improve the wear resistance of the base fabric.

Benefits of technology

The production process is green and environmentally friendly, and the wear resistance of the base fabric is significantly improved, meeting the wear resistance requirements of basketball leather.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of synthetic leather base cloth, and provides a production method of water-based basketball leather base cloth, which solves the defects that the production process of the basketball leather base cloth in the prior art is not environment-friendly and the obtained basketball leather is poor in wear resistance, and comprises the following preparation processes: (1) preparing a non-woven fabric; the non-woven fabric is conveyed into an impregnation tank, impregnation liquid is placed in the impregnation tank in advance, the impregnation liquid contains modified waterborne polyurethane emulsion, and the weight ratio of the non-woven fabric to the impregnation liquid is 1: (8-20); (3) drying for the first time: feeding the non-woven fabric treated by the water-containing waterborne resin in the step (2) into a drying oven to be dried, and controlling the drying temperature to be 140-170 DEG C; (4) coating water-based foaming resin slurry, wherein the foaming ratio of the water-based foaming resin slurry is 1.2-1.9, and the viscosity of the water-based foaming resin slurry is 26-32 Pa s; and (5) drying for the second time to obtain the water-based basketball leather base cloth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of synthetic leather base fabrics, in particular to a production method of a water-based basketball leather base fabric. Background Art

[0002] Solvent-based polyurethane contains many organic solvents, which are easy to volatilize. The traditional basketball leather base fabric is made of solvent-based polyurethane resin that is first impregnated with non-woven fabric, and then produced through surface coating, coagulation, washing, drying and other processes. The entire production process is not environmentally friendly, and the base fabric has a high DMF content, which does not meet the requirements of green, low-carbon, environmentally friendly and DMF-free.

[0003] With the improvement of environmental regulations and the enhancement of people's environmental awareness, the existing technology uses environmentally friendly water-based polyurethane to replace traditional solvent-based polyurethane. However, the traditional water-based polyurethane impregnated base fabric generally has a softer performance and better elasticity, but the wear resistance is often insufficient. As a basketball leather, it is often required to have better wear resistance.

[0004] Chinese patent No. 200910185158.X discloses a method for producing super wear-resistant and high-elastic ball leather, which comprises selecting a base fabric with a difference of less than 20% in elongation in the warp and weft directions, coating the base fabric with a polyurethane coating to form a wet semi-finished product; selecting release paper, uniformly coating the front of the release paper with a mixed slurry having high resilience and high wear resistance, and drying to obtain a surface film; uniformly coating the surface film of the release paper with a two-liquid mixed slurry having a good degree of crosslinking, and drying to obtain a transfer film, laminating the transfer film of the release paper with the wet semi-finished product, and peeling the leather from the release paper after drying to obtain a super wear-resistant and high-elastic ball leather. The invented product can meet the requirements of high resilience, super wear resistance and waterproofness for competition balls, but the polyurethane coating coated on the base fabric contains a relatively high proportion of dimethylformamide, i.e., DMF, and the production process is relatively environmentally unfriendly. Summary of the invention

[0005] Therefore, in view of the above-mentioned problems, the present invention provides a method for producing a water-based basketball leather base cloth to solve the defects of the prior art that the production process of the basketball leather base cloth is not environmentally friendly and the obtained basketball leather has poor wear resistance.

[0006] To achieve the above object, the present invention adopts the following technical solution: a method for producing a water-based basketball leather base fabric, comprising the following preparation process: (1) Preparation of non-woven fabrics; (2) Impregnation with aqueous resin: the non-woven fabric is transported into an impregnation tank, in which an impregnation liquid is placed in advance, the impregnation liquid contains a modified aqueous polyurethane resin emulsion, and the weight ratio of the non-woven fabric to the impregnation liquid is 1:8-20; (3) First drying: the non-woven fabric treated with the water-based resin in step (2) is placed in an oven for drying at a temperature of 140-170°C; (4) coating water-based foaming resin slurry: the water-based foaming resin slurry has a foaming ratio of 1.2-1.9 and a viscosity of 26-32 Pa˙s; (5) Drying for the second time to obtain the water-based basketball leather base fabric.

[0007] Further: The specific method of the second drying in step (5) is: first raise the temperature to 50-130°C, maintain for 2-8 minutes, and then raise the temperature to 130-160°C, maintain for 5-15 minutes.

[0008] Further: the preparation process of the modified waterborne polyurethane resin emulsion is as follows: (1) preparing raw materials: 70-80 parts by weight of polycarbonate diol, 20-50 parts by weight of isophorone diisocyanate, 5-15 parts by weight of 2,2-dimethylol propionic acid, 1-1.3 parts by weight of crosslinking agent trimethylolpropane, 5-20 parts by weight of triethylamine, 3-6 parts by weight of silane coupling agent KH-602, and 0.3-1.5 parts by weight of catalyst DBTDL; (2) mixing polycarbonate diol and 2,2-dimethylol propionic acid, stirring evenly at 46-50°C under nitrogen protection, adding IPDI isophorone diisocyanate and catalyst, heating to 60-65°C, and reacting 1-1.2h, then heat to 80-85℃, react for 2-3h, then add 1-1.3 parts of crosslinking agent trimethylolpropane, react at 80-85℃ for 2-2.5h, measure the isocyanate content, and when R value = 1.3-1.7, cool to 38-42℃, then add triethylamine, react for 20-30min, add acetone during the reaction to adjust the viscosity, and obtain a waterborne polyurethane prepolymer; (3) add deionized water to the waterborne polyurethane prepolymer, continue stirring, heat to 38-42℃, add hydrazine hydrate, react for 30-40min, then cool to 18-20℃, add silane coupling agent KH-602, and obtain a modified waterborne polyurethane emulsion.

[0009] Furthermore, the preparation process of the water-based resin foaming slurry includes: mixing 100 parts by weight of water-based polyurethane foaming resin, 1-3 parts by weight of dispersant, and 2-5 parts by weight of foaming agent, dispersing for 5-10 minutes, adding 100 parts by weight of silicon dioxide nanoparticles, continuing to stir until uniform, then blowing air into the mixture for foaming, and slowly adding thickener multiple times to adjust the viscosity to 26-32 Pa˙s.

[0010] Further: the dispersant is a nonionic dispersant, a zwitterionic dispersant or a polymer dispersant.

[0011] Further: the foaming agent is a uric acid foaming agent.

[0012] Furthermore: the thickener is an acrylic thickener.

[0013] Furthermore: the amount of the thickener is 1-10 parts by weight.

[0014] Furthermore: the non-woven fabric is a non-woven needle-punched non-woven fabric.

[0015] Furthermore, 10-20 parts by weight of nitrile rubber is added to the water-based resin foaming slurry.

[0016] By adopting the above technical solution, the beneficial effects of the present invention are: 1. The present invention uses water-based resin to impregnate non-woven fabric, and after drying, it is coated with water-based foaming resin and dried again to produce water-based basketball leather base fabric. The process is simple in production process, and the base fabric produced does not contain DMF, is green, low-carbon and environmentally friendly.

[0017] 2. The present invention uses modified waterborne polyurethane resin emulsion to impregnate nonwoven fabrics. The waterborne polyurethane resin is modified to obtain a base fabric with high wear resistance.

[0018] 3. In the preparation process of the modified waterborne polyurethane resin emulsion of the present invention, polycarbonate diol is selected as the main raw material of the prepolymer. The hard segment of the polycarbonate diol prepolymer accounts for a relatively high proportion, the intermolecular force is relatively large, the molecular chain is tightly bound, water is difficult to penetrate, the water absorption rate is reduced, and the particles are not easy to collapse during the film forming process, forming a rough surface, which is conducive to improving its wear resistance. Polycarbonate diol contains a large number of carbonate groups, which are highly polar and help to form hydrogen bonds.

[0019] 4. The crosslinking agent trimethylolpropane used has three hydroxyl groups on the molecule, which can react with the isocyanate on isophorone diisocyanate to crosslink the waterborne polyurethane molecular chains to form a crosslinked polymer.

[0020] 5. During the preparation process, the R value is controlled at 1.3-1.7, R value = nNCO / nOH. The smaller the R value, the greater the viscosity of the synthesized prepolymer, because the molecular weight of the prepolymer is larger. If the viscosity is too high, it is not easy to emulsify, and acetone needs to be added to reduce the viscosity. The present invention controls the R value within a suitable range, and a product with higher wear resistance can be obtained.

[0021] 6. During the preparation process, the chain extender is selected as silane coupling agent KH-602, which can improve the surface roughness of the material and thus enhance the wear resistance.

[0022] 7. Silica nanoparticles are added in the preparation process of water-based resin foaming slurry to further improve the wear resistance of the material. DETAILED DESCRIPTION

[0023] Embodiment 1

[0024] A method for producing a water-based basketball leather base fabric comprises the following preparation processes: (1) Preparation of non-woven fabrics: Nylon and polyester fibers are used as the main components and non-woven fabrics are prepared by a web-laying needle punching method; (2) Water-based resin impregnation treatment: the non-woven fabric is transported into an impregnation tank, in which an impregnation liquid is placed in advance, the impregnation liquid contains a modified waterborne polyurethane resin emulsion, and the weight ratio of the non-woven fabric to the impregnation liquid is 1:8; the preparation process of the modified waterborne polyurethane resin emulsion is as follows: a. Preparation of raw materials: 70 parts by weight of polycarbonate diol, 20 parts by weight of isophorone diisocyanate, 5 parts by weight of 2,2-dimethylolpropionic acid, 1 part of cross-linking agent trimethylolpropane, 5 parts by weight of triethylamine, 3 parts by weight of silane coupling agent KH-602, and 0.3 parts by weight of catalyst DBTDL; b. Mix polycarbonate diol and 2,2-dimethylolpropionic acid, and heat at 4 6°C and stirred evenly under nitrogen protection, isophorone diisocyanate and catalyst were added, the temperature was raised to 60°C, the reaction was continued for 1 hour, the temperature was raised to 80°C, the reaction was continued for 2 hours, 1 part of cross-linking agent trimethylolpropane was added, the reaction was continued at 80°C for 2 hours, the isocyanate content was determined, and when the R value was 1.3, the temperature was lowered to 38°C, triethylamine was added, the reaction was continued for 20 minutes, acetone was added during the reaction to adjust the viscosity, and a waterborne polyurethane prepolymer was obtained; c. deionized water was added to the waterborne polyurethane prepolymer, the mixture was stirred continuously, the temperature was raised to 38°C, hydrazine hydrate was added, the reaction was continued for 30 minutes, the temperature was lowered to 18°C, silane coupling agent KH-602 was added, and a modified waterborne polyurethane emulsion was obtained; (3) First drying: the non-woven fabric treated with the aqueous resin in step (2) is placed in an oven for drying at a temperature of 140°C; (4) Coating water-based foaming resin slurry: The foaming ratio of the water-based foaming resin slurry is 1.2. The preparation process of the water-based resin foaming slurry includes: mixing 100 parts by weight of water-based polyurethane foaming resin, 1 part by weight of dispersant, and 2 parts by weight of uric acid foaming agent, dispersing for 5 minutes, adding 100 parts by weight of silica nanoparticles, continuing to stir until uniform, then blowing air into the mixture for foaming, and slowly adding acrylic thickener several times to make the viscosity reach 26 Pa˙s; the amount of the thickener used is 5 parts by weight; (5) Drying for the second time to obtain a water-based basketball leather base fabric. The specific method of the second drying is: first heating to 50°C, maintaining for 8 minutes, and then heating to 130°C, maintaining for 15 minutes.

[0025] Embodiment 2

[0026] A method for producing a water-based basketball leather base fabric comprises the following preparation processes: (1) Preparation of non-woven fabrics; (2) Impregnation with water-based resin: The non-woven fabric is transported into an impregnation tank, in which an impregnation liquid is placed in advance, wherein the impregnation liquid contains a modified water-based polyurethane resin emulsion, and the weight ratio of the non-woven fabric to the impregnation liquid is 1:15; the preparation process of the modified water-based polyurethane resin emulsion is as follows: a. Preparation of raw materials: 75 parts by weight of polycarbonate diol, 35 parts by weight of isophorone diisocyanate, 10 parts by weight of 2,2-dimethylolpropionic acid, 1.2 parts by weight of cross-linking agent trimethylolpropane, 15 parts by weight of triethylamine, 5 parts by weight of silane coupling agent KH-602, and 1 part by weight of catalyst DBTDL; b. Mix polycarbonate diol and 2,2-dimethylolpropionic acid, and heat at 48°C. and nitrogen protection environment, stirring evenly, adding isophorone diisocyanate and catalyst, heating to 62°C, reacting for 1.1h, then heating to 82°C, reacting for 2.5h, then adding 1.2 parts of cross-linking agent trimethylolpropane, reacting at 83°C for 2.2h, measuring the isocyanate content, and when the R value = 1.5, cooling to 40°C, adding triethylamine, reacting for 25min, adding acetone during the reaction to adjust the viscosity, and obtaining a waterborne polyurethane prepolymer; c, adding deionized water to the waterborne polyurethane prepolymer, stirring continuously, heating to 40°C, adding hydrazine hydrate to react for 35min, then cooling to 19°C, adding silane coupling agent KH-602, and obtaining a modified waterborne polyurethane emulsion; (3) First drying: the non-woven fabric treated with the aqueous resin in step (2) is placed in an oven for drying, and the drying temperature is controlled at 155°C; (4) Coating water-based foaming resin slurry: The foaming ratio of the water-based foaming resin slurry is 1.6. The preparation process of the water-based resin foaming slurry includes: mixing 100 parts by weight of water-based polyurethane foaming resin, 15 parts by weight of nitrile rubber, 2 parts by weight of dispersant, and 3 parts by weight of uric acid foaming agent, dispersing for 7 minutes, adding 100 parts by weight of silica nanoparticles, continuing to stir until uniform, then blowing air into the mixture for foaming, and slowly adding acrylic thickener several times to make the viscosity reach 30 Pa˙s; the amount of thickener used is 8 parts by weight; The silicon dioxide nanoparticles are synthesized from tetraethoxysilane by a sol-gel method to SiO2˙, and methyltriethoxysilane is added during the synthesis process to modify the surface of SiO2, so that the modified SiO2 nanoparticles are more evenly distributed in the emulsion and have better wear resistance; (5) Drying for the second time to obtain the water-based basketball leather base fabric is first heated to 100°C and maintained for 6 min, then heated to 150°C and maintained for 10 min.

[0027] Embodiment 3

[0028] A method for producing a water-based basketball leather base fabric comprises the following preparation processes: (1) Preparation of nonwoven needle-punched nonwoven fabrics; (2) Impregnation with water-based resin: The ultrafine fiber non-woven fabric is transported into an impregnation tank, in which an impregnation liquid is placed in advance, wherein the impregnation liquid contains a modified water-based polyurethane resin emulsion, and the weight ratio of the non-woven fabric to the impregnation liquid is 1:20; the preparation process of the modified water-based polyurethane resin emulsion is as follows: a. Preparation of raw materials: 80 parts by weight of polycarbonate diol, 50 parts by weight of isophorone diisocyanate, 15 parts by weight of 2,2-dimethylolpropionic acid, 1.3 parts by weight of cross-linking agent trimethylolpropane, 20 parts by weight of triethylamine, 6 parts by weight of silane coupling agent KH-602, and 1.5 parts by weight of catalyst DBTDL; b. Mix polycarbonate diol and 2,2-dimethylolpropionic acid at 50 ℃ and nitrogen protection environment, stir evenly, add IPDI isophorone diisocyanate and catalyst, heat to 65℃, react for 1.2h, then heat to 85℃, react for 3h, then add 1.3 parts of cross-linking agent trimethylolpropane, react at 85℃ for 2.5h, measure the isocyanate content, when R value = 1.7, cool to 42℃, add triethylamine, react for 30min, add acetone to adjust viscosity during the reaction, and obtain a waterborne polyurethane prepolymer; c, add deionized water to the waterborne polyurethane prepolymer, keep stirring, heat to 42℃, add hydrazine hydrate to react for 40min, then cool to 20℃, add silane coupling agent KH-602, and obtain a modified waterborne polyurethane emulsion; (3) First drying: the non-woven fabric treated with the aqueous resin in step (2) is placed in an oven for drying at a temperature of 170°C; (4) Coating water-based foaming resin slurry: The foaming ratio of the water-based foaming resin slurry is 1.9. The preparation process of the water-based resin foaming slurry includes: mixing 100 parts by weight of water-based polyurethane foaming resin, 3 parts by weight of dispersant, and 5 parts by weight of AC foaming agent, dispersing for 10 minutes, adding 100 parts by weight of heavy calcium powder, continuing to stir until uniform, then blowing air into the mixture for foaming, and slowly adding acrylic thickener several times to make the viscosity reach 2Pa˙s; the amount of thickener used is 10 parts by weight; (5) Drying for the second time to obtain the water-based basketball leather base fabric, first heat it to 130°C and keep it for 8 minutes, then heat it to 160°C and keep it for 15 minutes.

[0029] The dispersant of the present invention is a nonionic dispersant, a zwitterionic dispersant or a polymer dispersant. The dispersants are all commercially available well-known products and will not be described in detail here. The purpose of the present invention can be achieved by selecting any one of them.

[0030] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes may be made to the present invention in form and details without departing from the spirit and scope of the present invention as defined by the appended claims, all of which are within the scope of protection of the present invention.

Claims

1. A method for producing a water-based basketball leather base fabric, characterized in that: The preparation process includes the following: (1) Preparation of non-woven fabrics; (2) Impregnation with aqueous resin: the non-woven fabric is transported into an impregnation tank, in which an impregnation liquid is placed in advance, the impregnation liquid contains a modified aqueous polyurethane resin emulsion, and the weight ratio of the non-woven fabric to the impregnation liquid is 1:8-20; (3) First drying: the non-woven fabric treated with the water-based resin in step (2) is placed in an oven for drying at a temperature of 140-170°C; (4) coating water-based foaming resin slurry: the water-based foaming resin slurry has a foaming ratio of 1.2-1.9 and a viscosity of 26-32 Pa˙s; (5) Drying for the second time to obtain the water-based basketball leather base fabric.

2. The method for producing a water-based basketball leather base fabric according to claim 1, characterized in that: The specific method of the second drying in step (5) is: first raise the temperature to 50-130°C, maintain for 2-8 minutes, and then raise the temperature to 130-160°C, maintain for 5-15 minutes.

3. The method for producing a water-based basketball leather base fabric according to claim 1, characterized in that: The preparation process of the modified waterborne polyurethane resin emulsion is as follows: (1) preparing raw materials: 70-80 parts by weight of polycarbonate diol, 20-50 parts by weight of isophorone diisocyanate, 5-15 parts by weight of 2,2-dimethylol propionic acid, 1-1.3 parts by weight of crosslinking agent trimethylolpropane, 5-20 parts by weight of triethylamine, 3-6 parts by weight of silane coupling agent KH-602, and 0.3-1.5 parts by weight of catalyst DBTDL; (2) mixing polycarbonate diol and 2,2-dimethylol propionic acid, stirring evenly at 46-50° C. under nitrogen protection, adding isophorone diisocyanate and catalyst, heating to 60-65° C., reacting for 1-1. 2h, then heat to 80-85℃, react for 2-3h, then add 1-1.3 parts of cross-linking agent trimethylolpropane, react at 80-85℃ for 2-2.5h, measure the isocyanate content, and when R value = 1.3-1.7, cool to 38-42℃, then add triethylamine, react for 20-30min, add acetone during the reaction to adjust the viscosity, and obtain a waterborne polyurethane prepolymer; (3) add deionized water to the waterborne polyurethane prepolymer, continue stirring, heat to 38-42℃, add hydrazine hydrate, react for 30-40min, then cool to 18-20℃, add silane coupling agent KH-602, and obtain a modified waterborne polyurethane emulsion.

4. The method for producing a water-based basketball leather base fabric according to claim 3, characterized in that: The preparation process of the water-based resin foaming slurry comprises: mixing 100 parts by weight of water-based polyurethane foaming resin, 1-3 parts by weight of dispersant, and 2-5 parts by weight of foaming agent, dispersing for 5-10 minutes, adding 100 parts by weight of silicon dioxide nanoparticles, stirring until uniform, blowing air into the slurry for foaming, and slowly adding thickener multiple times to make the viscosity reach 26-32 Pa˙s.

5. The method for producing a water-based basketball leather base fabric according to claim 4, characterized in that: The dispersant is a nonionic dispersant, a zwitterionic dispersant or a polymer dispersant.

6. The method for producing a water-based basketball leather base fabric according to claim 4, characterized in that: The foaming agent is a uric acid foaming agent.

7. The method for producing a water-based basketball leather base fabric according to claim 4, characterized in that: The thickener is an acrylic thickener.

8. The method for producing a water-based basketball leather base fabric according to claim 4, characterized in that: The amount of the thickener is 1-10 parts by weight.

9. The method for producing a water-based basketball leather base fabric according to claim 1, characterized in that: The non-woven fabric is a non-woven needle-punched non-woven fabric.

10. The method for producing a water-based basketball leather base fabric according to claim 4, characterized in that: 10-20 parts by weight of nitrile rubber is also added to the water-based resin foaming slurry.