Paper-based facing material with anti-ultraviolet function and preparation method thereof
By using titanium dioxide-loaded calcium carbonate fillers and surfactants and other materials in paper-based finish materials, combined with pulping and glue filling processes, the problem of insufficient UV resistance performance of paper-based finish materials is solved, and more efficient resistance is achieved UV absorption and sterilization effect.
Patent Information
- Application Number
- CN202411218905.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing paper-based finishing materials have insufficient UV resistance, making it difficult to meet the needs of building materials products for functions such as UV protection and sterilization.
Use pulping of surfactant, calcium carbonate filler and wood pulp to prepare glue sizing agents by enzymatic dissolving of starch and aluminum sulfate and other materials, and loading titanium dioxide into calcium carbonate filler, and pulping, squeezing, pressing, and applying The paper-based finishing materials were prepared by other processes, and the photochemical reaction of titanium dioxide was used to enhance the resistance to UV.
It improves the UV resistance of paper-based finish materials, enhances its absorption and bactericidal ability to ray ultraviolet rays, and ensures that a small amount of titanium dioxide can exert an efficient UV resistance effect at the nanoscale.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of papermaking, and in particular to a paper-based finishing material with anti-ultraviolet function and a preparation method thereof. Background Art
[0002] Paper-based finishing materials are a type of industrial specialty paper processed through a special process. They are also an indispensable raw material in many building materials products, such as low-pressure boards and high-pressure boards used in furniture and cabinets, as well as fireproof boards, floors, wallpapers, etc., which all require paper-based finishing materials to enhance the aesthetics of the products.
[0003] Paper-based finishing materials are usually manufactured through pulping, papermaking, pressing and other processes. Anti-ultraviolet performance is one of the important properties to measure the quality of paper-based finishing materials. How to improve the anti-ultraviolet effect of paper-based finishing materials is a technical problem that technicians in this field are currently committed to solving. Summary of the invention
[0004] One of the problems solved by the present invention is how to provide a paper-based finishing material with good anti-ultraviolet effect.
[0005] In order to solve at least one of the above problems, the present invention provides a method for preparing a paper-based facing material with anti-ultraviolet function, the preparation method comprising:
[0006] S100, mixing raw materials including a surfactant, a calcium carbonate filler and wood pulp to obtain pulp;
[0007] S200, placing the pulp on the screen for papermaking, pressing, and drying to obtain base paper;
[0008] S300, applying sizing agent to base paper, drying and calendering to obtain paper-based finishing material;
[0009] The porous calcium carbonate filler is loaded with titanium dioxide.
[0010] In any of the above technical solutions, the surfactant includes at least one of the following or a combination thereof: sodium dodecylbenzene sulfonate, sodium tetrapropylenebenzene sulfonate, sodium fatty alcohol sulfate, xylene sulfonic acid, and condensed sodium naphthalene sulfonate.
[0011] In any of the above technical solutions, the sizing agent is prepared by the following steps:
[0012] S111, using α-amylase to enzymatically hydrolyze starch to obtain enzymatically hydrolyzed starch;
[0013] S112, mixing the defoaming agent, aluminum sulfate, styrene-acrylate copolymer and enzymatic starch, and adding water to prepare a sizing agent with a solid content of 28% to 32% and a pH value of 4.5 to 5.
[0014] In any of the above technical solutions, in S111, the starch is cereal starch or rhizome starch.
[0015] In any of the above technical solutions, the dosage of α-amylase is 200 ppm to 400 ppm based on the amount of starch added.
[0016] In any of the above technical schemes, the enzymatic treatment method is: α-amylase and starch are mixed and sent into a reactor, 2 to 2.5 times the mass of starch is added with water, and the mixture is reacted for 20 to 30 minutes at a temperature of 75°C to 85°C and a pressure of 40,000 Pa to 55,000 Pa, and the solids are extracted and dried at a temperature of 120°C to 130°C.
[0017] In any of the above technical solutions, in S112, the mass ratio of defoaming agent: aluminum sulfate: styrene-acrylate copolymer: enzymatic starch = (0.5-1): (0.5-1): (40-60): 100.
[0018] In any of the above technical solutions, the calcium carbonate filler is prepared by the following steps:
[0019] S121, mixing titanium tetrachloride and calcium carbonate in water and stirring to obtain a first mixture;
[0020] S122, mixing sodium dodecylbenzene sulfonate and sodium hydroxide in water and stirring to obtain a second mixture;
[0021] S123, mixing the first mixture and the second mixture to react to obtain calcium carbonate.
[0022] In any of the above technical solutions, in S121, the mass ratio of titanium tetrachloride: calcium carbonate: water = (4-6): (14-16): 100.
[0023] In any of the above technical solutions, in S122, the mass ratio of sodium dodecylbenzenesulfonate: sodium hydroxide: water = (0.5-1): (4-8): 100.
[0024] In any of the above technical solutions, S123 specifically includes:
[0025] The second mixture is added dropwise into the first mixture with stirring until the pH value is 10-11. After the addition is completed, the mixture is allowed to stand for 20 to 30 minutes, the solids are filtered, washed, dried, and heat treated at a temperature of 650 to 680° C. for 1 to 1.5 hours to obtain calcium carbonate.
[0026] The present invention also provides a paper-based decorative material with anti-ultraviolet function. The paper-based decorative material with anti-ultraviolet function is obtained by adopting the preparation method of any of the above technical solutions.
[0027] Beneficial Effects
[0028] The present invention provides a method for preparing a paper-based facing material with an anti-ultraviolet function. The method firstly uses raw materials including a surfactant, a calcium carbonate filler and wood pulp to mix and pulp to obtain a pulp; then the pulp is put on a net for papermaking, pressing and drying to obtain a base paper; finally, a sizing agent is used to sizing the base paper, drying and calendering to obtain a paper-based facing material. The porous calcium carbonate filler is loaded with titanium dioxide.
[0029] The present invention adds titanium dioxide to the slurry and uses the characteristic of absorbing ultraviolet rays to give the paper-based finishing material anti-ultraviolet properties. When titanium dioxide is irradiated with ultraviolet rays, the electrons in its electronic structure will be excited and jump from the valence band to the conduction band to form photogenerated electrons and photogenerated holes. These photogenerated electrons and holes have reducing and oxidizing properties respectively and can react with substances adsorbed on the surface. This photochemical reaction not only helps to enhance the anti-ultraviolet ability of titanium dioxide, but also gives it multiple functions such as sterilization and degradation of organic matter.
[0030] On this basis, the present invention chooses to load titanium dioxide on calcium carbonate to achieve anti-ultraviolet effect with calcium carbonate filler containing titanium dioxide. The advantage is that it can avoid the agglomeration of nano-scale titanium dioxide with smaller particle size in the slurry, ensuring that a smaller amount of titanium dioxide can play a better and more efficient anti-ultraviolet effect. DETAILED DESCRIPTION
[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the following is a detailed description of the specific embodiments of the present invention.
[0032] Unless otherwise specified, the reagents and raw materials used in the present invention can be purchased through commercial channels. The experimental methods in the following examples without specifying specific conditions are selected according to conventional methods and conditions, or according to the product specifications.
[0033] Paper-based finishing materials can be used in a variety of application scenarios such as furniture veneer and wallpaper. Anti-ultraviolet performance is one of the important properties to measure the quality of paper-based finishing materials. How to improve the anti-ultraviolet performance of paper-based finishing materials has always been a technical problem that technicians in this field have been committed to solving.
[0034] In order to solve the above problems, an embodiment of the present invention provides a method for preparing a paper-based facing material with anti-ultraviolet function, the preparation method comprising:
[0035] S100, mixing raw materials including a surfactant, a calcium carbonate filler and wood pulp to obtain pulp;
[0036] S200, placing the pulp on the screen for papermaking, pressing, and drying to obtain base paper;
[0037] S300, applying sizing agent to base paper, drying and calendering to obtain paper-based finishing material;
[0038] The porous calcium carbonate filler is loaded with titanium dioxide.
[0039] The technical solution of the present invention is suitable for preparing indoor decoration paper such as furniture veneer, wallpaper, etc. Titanium dioxide imparts anti-ultraviolet properties to the paper-based finishing material.
[0040] The surfactant includes at least one of the following or a combination thereof: sodium dodecylbenzene sulfonate, sodium tetrapropylenebenzene sulfonate, sodium fatty alcohol sulfate, xylene sulfonic acid, and condensed sodium naphthalene sulfonate.
[0041] Preferably, the wood pulp used in S100 includes white coniferous wood pulp and bleached broadleaf wood pulp in a mass ratio of (0.25-0.5):1.
[0042] The paper-based facing material of the present invention is mainly manufactured by pulping, papermaking, pressing and other processes. Those skilled in the art can select and adjust the equipment, raw materials and process parameters used in pulping, papermaking and pressing according to actual needs.
[0043] Pulping is a key process in the papermaking industry, which separates the fibers from the plant fiber raw materials to obtain paper pulp. The pulping step of the present invention can be carried out by mechanical method, chemical method or chemical mechanical method. The papermaking step uses a bamboo curtain type mesh trough specially used for papermaking to scoop a certain amount of paper pulp, and then swings the mesh trough back and forth or left and right to arrange the pulp fibers in a certain direction to form a paper layer of uniform thickness, i.e., wet paper sheet. The pressing process squeezes the wet paper through a press, which removes excess water from the paper layer and increases the dryness of the paper. The pressure and speed in the pressing process can be selected and adjusted by those skilled in the art according to actual needs.
[0044] It can be understood that the process of using pulp to make paper on the net, press and dry to obtain base paper is a relatively mature existing technology. The selection of specific process parameters for making paper on the net, press and dry has no substantial impact on the realization of the purpose of the present invention.
[0045] Preferably, the beating degree of the wood pulp used in S100 is 30°SR to 45°SR.
[0046] Preferably, in S100, the mass ratio of surfactant: calcium carbonate filler: wood pulp = (1-2): (10-15): 100.
[0047] Further, preferably, in S100, the mass ratio of surfactant: calcium carbonate filler: wood pulp is 1.5:12:100.
[0048] Regarding S300, the purpose of sizing is to enhance the anti-permeability of the paper-based finishing material so that the paper-based finishing material can better resist the penetration of liquids such as water and grease, thereby keeping it dry and tidy. In addition, the sizing agent can form a protective film on the surface of the paper-based finishing material, which helps to prevent it from tearing and wrinkling, thereby improving the strength and stability of the paper. The present invention selects the method of surface sizing for sizing, that is: spraying a thin layer of sizing agent on the surface of the paper-based finishing material to form a protective film on the surface of the base paper. The surface sizing process of the present invention is carried out on a papermaking machine. The present invention can use starch, animal glue, synthetic glue and other materials as sizing agents. The amount of sizing agent can be selected and adjusted by those skilled in the art. Preferably, the sizing agent of the present invention is prepared by the following steps:
[0049] S111, using α-amylase to enzymatically hydrolyze starch to obtain enzymatically hydrolyzed starch;
[0050] S112, mixing the defoaming agent, aluminum sulfate, styrene-acrylate copolymer and enzymatic starch, and adding water to prepare a sizing agent with a solid content of 28% to 32% and a pH value of 4.5 to 5.
[0051] Specifically, in S111, the starch is cereal starch or rhizome starch, and the amount of α-amylase used is 200ppm to 400ppm based on the amount of starch added; the enzymatic treatment method is: the α-amylase and starch are mixed and sent into a reactor, 2 to 2.5 times the mass of starch is added with water, and the mixture is reacted for 20 to 30 minutes at a temperature of 75°C to 85°C and a pressure of 40000Pa to 55000Pa, and the solids are extracted and dried at a temperature of 120°C to 130°C.
[0052] Preferably, in S111, the amount of α-amylase used is 200 ppm based on the amount of starch added; the enzymatic treatment method is: the α-amylase and starch are mixed and sent into a reactor, water twice the mass of the starch is added, and the reaction is carried out at a temperature of 80°C and a pressure of 50,000 Pa for 20 minutes, and the solids are extracted and dried at a temperature of 125°C.
[0053] Preferably, in S112, the mass ratio of defoaming agent: aluminum sulfate: styrene-acrylate copolymer: enzymatic starch is (0.5-1): (0.5-1): (40-60): 100.
[0054] More preferably, in S112, the mass ratio of defoaming agent: aluminum sulfate: styrene-acrylate copolymer: enzymatic starch is 0.5:1:40:100.
[0055] One of the improvements made by the present invention over the prior art is to load titanium dioxide on calcium carbonate to achieve an anti-ultraviolet effect with a calcium carbonate filler containing titanium dioxide. The advantage is that it can prevent the agglomeration of nano-scale titanium dioxide with a smaller particle size in the slurry, ensuring that a better and more efficient anti-ultraviolet effect is achieved with a smaller amount of titanium dioxide. Specifically, the calcium carbonate filler used in the present invention is prepared by the following steps:
[0056] S121, mixing titanium tetrachloride and calcium carbonate in water and stirring to obtain a first mixture;
[0057] S122, mixing sodium dodecylbenzene sulfonate and sodium hydroxide in water and stirring to obtain a second mixture;
[0058] S123, mixing the first mixture and the second mixture to react to obtain calcium carbonate.
[0059] Optionally, in S121, the mass ratio of titanium tetrachloride:calcium carbonate:water=(4-6):(14-16):100.
[0060] Optionally, in S122, the mass ratio of sodium dodecylbenzenesulfonate:sodium hydroxide:water=(0.5-1):(4-8):100.
[0061] Preferably, in S122, the mass ratio of sodium dodecylbenzene sulfonate: sodium hydroxide: water is 1:5:100.
[0062] In the present invention, S123 specifically includes:
[0063] The second mixture is added dropwise into the first mixture with stirring until the pH value is 10-11. After the addition is completed, the mixture is allowed to stand for 20 to 30 minutes, the solids are filtered, washed, dried, and heat treated at a temperature of 650 to 680° C. for 1 to 1.5 hours to obtain calcium carbonate.
[0064] Through the above steps, the present invention first mixes titanium tetrachloride and calcium carbonate in water to obtain a first mixture. Then, sodium dodecylbenzene sulfonate and sodium hydroxide as surfactants are mixed and stirred in water to obtain a second mixture as an alkaline solution. By dropping the second mixture into the first mixture and stirring it simultaneously, and letting it stand after the dropwise addition is completed, titanium tetrachloride can produce titanium hydroxide under alkaline conditions, and a titanium hydroxide coating layer is deposited on the surface of calcium carbonate. Finally, the present invention oxidizes titanium hydroxide into titanium dioxide through heat treatment at a temperature of 650°C to 680°C.
[0065] Example 1
[0066] This embodiment provides a paper-based facing material with anti-ultraviolet function, which is prepared by the following steps:
[0067] S1. Mix titanium tetrachloride and calcium carbonate in water in a mass ratio of titanium tetrachloride: calcium carbonate: water = 6:15:100 to obtain a first mixture;
[0068] S2, mixing sodium dodecylbenzene sulfonate and sodium hydroxide in water in a mass ratio of sodium dodecylbenzene sulfonate: sodium hydroxide: water = 1:6:100 to obtain a second mixture;
[0069] S3, adding the second mixture dropwise into the first mixture and stirring simultaneously until the pH value is 10-11, adjusting and standing for 20 minutes after the addition is completed, filtering the solid, washing with water twice, drying, and heat treating at a temperature of 660° C. for 1.5 hours to obtain a calcium carbonate filler;
[0070] S4, mixing α-amylase and starch into a reactor, adding water twice the mass of starch, reacting for 20 min at a temperature of 80° C. to 85° C. and a pressure of 45000 Pa to 55000 Pa, extracting the solids and drying them at a temperature of 125±3° C.; wherein, based on the amount of starch added, the amount of α-amylase used is 200 ppm;
[0071] S5, according to the mass ratio of polyether defoamer: aluminum sulfate: styrene-acrylate copolymer: enzymatic starch = 0.5:1:40:100, the polyether defoamer, aluminum sulfate, styrene-acrylate copolymer and enzymatic starch are mixed, and water is added to prepare a sizing agent with a solid content of 30% and a pH value of 4.5 to 5;
[0072] S6. Mixing raw materials including sodium dodecylbenzene sulfonate, calcium carbonate filler, bleached coniferous pulp and bleached broadleaf pulp in a mass ratio of sodium dodecylbenzene sulfonate: calcium carbonate filler: bleached coniferous pulp: bleached broadleaf pulp = 1.5:3:12:30:70 to obtain a pulp having a beating degree of about 35° SR;
[0073] S7, placing the pulp on the screen for papermaking, pressing, and drying to obtain base paper;
[0074] S8. Use a sizing agent with a mass of 4% of the mass of the base paper to sizing the base paper, dry and calender, and obtain a paper-based facing material.
[0075] Example 2
[0076] This embodiment provides a paper-based facing material with anti-ultraviolet function, which is prepared by the following steps:
[0077] S1. Mix titanium tetrachloride and calcium carbonate in water in a mass ratio of titanium tetrachloride: calcium carbonate: water = 4:16:100 to obtain a first mixture;
[0078] S2, mixing sodium dodecylbenzene sulfonate and sodium hydroxide in water in a mass ratio of sodium dodecylbenzene sulfonate: sodium hydroxide: water = 0.5:4:100, to obtain a second mixture;
[0079] S3, adding the second mixture dropwise into the first mixture and stirring simultaneously until the pH value is 10-11, adjusting and standing for 30 minutes after the addition is completed, filtering the solid, washing with water twice, drying, and heat treating at a temperature of 680° C. for 1 hour to obtain a calcium carbonate filler;
[0080] S4, mixing α-amylase and starch into a reactor, adding 2.5 times the mass of water of starch, reacting for 20 minutes at a temperature of 80°C to 85°C and a pressure of 45000Pa to 55000Pa, extracting the solids and drying them at a temperature of 125±3°C; wherein, based on the amount of starch added, the amount of α-amylase used is 400ppm;
[0081] S5, according to the mass ratio of polyether defoamer: aluminum sulfate: styrene-acrylate copolymer: enzymatic starch = 0.5:1:60:100, the polyether defoamer, aluminum sulfate, styrene-acrylate copolymer and enzymatic starch are mixed, and water is added to prepare a sizing agent with a solid content of 30% and a pH value of 4.5 to 5;
[0082] S6. Mixing raw materials including sodium dodecylbenzene sulfonate, calcium carbonate filler, bleached coniferous pulp and bleached broadleaf pulp in a mass ratio of sodium dodecylbenzene sulfonate: calcium carbonate filler: bleached coniferous pulp: bleached broadleaf pulp = 1.5:3:12:30:70 to obtain a pulp having a beating degree of about 35° SR;
[0083] S7, placing the pulp on the screen for papermaking, pressing, and drying to obtain base paper;
[0084] S8. Use a sizing agent with a mass of 4% of the mass of the base paper to sizing the base paper, dry and calender, and obtain a paper-based facing material.
[0085] Example 3
[0086] This embodiment provides a paper-based facing material with anti-ultraviolet function, which is prepared by the following steps:
[0087] S1. Mix α-amylase and starch into a reactor, add water twice the mass of starch, react for 20 min at a temperature of 80° C. to 85° C. and a pressure of 45000 Pa to 55000 Pa, extract the solid and dry it at a temperature of 125±3° C.; wherein, based on the amount of starch added, the amount of α-amylase used is 200 ppm;
[0088] S2, according to the mass ratio of polyether defoamer: aluminum sulfate: styrene-acrylate copolymer: enzymatic starch = 0.5:1:40:100, the polyether defoamer, aluminum sulfate, styrene-acrylate copolymer and enzymatic starch are mixed, and water is added to prepare a sizing agent with a solid content of 30% and a pH value of 4.5 to 5;
[0089] S3, mixing raw materials including sodium dodecylbenzene sulfonate, titanium dioxide, calcium carbonate filler, bleached coniferous pulp and bleached broadleaf pulp in a mass ratio of sodium dodecylbenzene sulfonate: titanium dioxide: calcium carbonate filler: bleached coniferous pulp: bleached broadleaf pulp = 1.5:2:10:30:70 to obtain a pulp having a beating degree of about 35° SR; wherein titanium dioxide and calcium carbonate filler are purchased through commercial channels;
[0090] S4, placing the pulp on the screen for papermaking, pressing, and drying to obtain base paper;
[0091] S5. Use a sizing agent with a mass of 4% of the mass of the base paper to sizing the base paper, dry and calender, and obtain a paper-based facing material.
[0092] Example 4
[0093] This embodiment provides a paper-based facing material, which is prepared by the following steps:
[0094] S1. Mix α-amylase and starch into a reactor, add water twice the mass of starch, react for 20 min at a temperature of 80° C. to 85° C. and a pressure of 45000 Pa to 55000 Pa, extract the solid and dry it at a temperature of 125±3° C.; wherein, based on the amount of starch added, the amount of α-amylase used is 200 ppm;
[0095] S2, according to the mass ratio of polyether defoamer: aluminum sulfate: styrene-acrylate copolymer: enzymatic starch = 0.5:1:40:100, the polyether defoamer, aluminum sulfate, styrene-acrylate copolymer and enzymatic starch are mixed, and water is added to prepare a sizing agent with a solid content of 30% and a pH value of 4.5 to 5;
[0096] S3, mixing raw materials including sodium dodecylbenzene sulfonate, calcium carbonate filler, bleached coniferous pulp and bleached broadleaf pulp in a mass ratio of sodium dodecylbenzene sulfonate: calcium carbonate filler: bleached coniferous pulp: bleached broadleaf pulp = 1.5:12:30:70 to obtain a pulp having a beating degree of about 35° SR; wherein the calcium carbonate filler is purchased through commercial channels;
[0097] S4, placing the pulp on the screen for papermaking, pressing, and drying to obtain base paper;
[0098] S5. Use a sizing agent with a mass of 4% of the mass of the base paper to sizing the base paper, dry and calender, and obtain a paper-based facing material.
[0099] Performance Testing
[0100] The paper-based facing materials of Examples 1-4 were cut into pieces of 50 mm × 50 mm, respectively, and placed in an aging box (light temperature 50° C., light intensity 800 w / m 2 ) for aging for 5 days, 10 days and 15 days, and a hue difference △E test was performed after the end of each time period. The test results are listed in the table below.
[0101] Hue difference △E 5 days 10 days 15 days Example 1 4.1 6.2 8.9 Example 2 4.0 6.3 8.7 Example 3 5.5 7.1 10.4 Example 4 6.9 9.0 13.5
Claims
1. A method for preparing a paper-based facing material with anti-ultraviolet function, characterized in that: The preparation method comprises: S100, mixing raw materials including a surfactant, a calcium carbonate filler and wood pulp to obtain pulp; S200, placing the slurry on a screen for papermaking, pressing, and drying to obtain base paper; S300, applying sizing agent to the base paper, drying and calendering to obtain the paper-based facing material; Wherein, the porous calcium carbonate filler is loaded with titanium dioxide.
2. The preparation method according to claim 1, characterized in that: The surfactant includes at least one of the following or a combination thereof: sodium dodecylbenzene sulfonate, sodium tetrapropylenebenzene sulfonate, sodium fatty alcohol sulfate, xylene sulfonic acid, and condensed sodium naphthalene sulfonate.
3. The preparation method according to claim 1, characterized in that: The sizing agent is prepared by the following steps: S111, using α-amylase to enzymatically hydrolyze starch to obtain enzymatically hydrolyzed starch; S112, mixing the defoaming agent, aluminum sulfate, styrene-acrylate copolymer and the enzymatically hydrolyzed starch, and adding water to prepare the sizing agent with a solid content of 28% to 32% and a pH value of 4.5 to 5.
4. The preparation method according to claim 3, characterized in that: In S111, the starch is cereal starch or rhizome starch.
5. The preparation method according to claim 3, characterized in that: In S111, the amount of α-amylase used is 200 ppm to 400 ppm based on the amount of starch added.
6. The preparation method according to claim 3, characterized in that: In S111, the enzymatic hydrolysis treatment method is: the α-amylase and the starch are mixed and sent into a reactor, 2 to 2.5 times the mass of the starch is added with water, the reaction is carried out at a temperature of 75°C to 85°C and a pressure of 40000Pa to 55000Pa for 20min to 30min, the solids are extracted and dried at a temperature of 120°C to 130°C.
7. The preparation method according to claim 3, characterized in that: In S112, the mass ratio of defoaming agent: aluminum sulfate: styrene-acrylate copolymer: enzymatic starch = (0.5-1): (0.5-1): (40-60):
100.
8. The preparation method according to any one of claims 1 to 5, characterized in that The calcium carbonate filler is prepared by the following steps: S121, mixing titanium tetrachloride and calcium carbonate in water and stirring to obtain a first mixture; S122, mixing sodium dodecylbenzene sulfonate and sodium hydroxide in water and stirring to obtain a second mixture; S123, mixing the first mixture and the second mixture to react, to obtain the calcium carbonate.
9. The preparation method according to claim 8, characterized in that: S123 specifically includes: The second mixture is added dropwise into the first mixture with simultaneous stirring until the pH value is 10-11. After the addition is completed, the mixture is allowed to stand for 20 to 30 minutes, the solid matter is filtered, washed, dried, and heat treated at a temperature of 650° C. to 680° C. for 1 hour to 1.5 hours to obtain the calcium carbonate.
10. A paper-based facing material with anti-ultraviolet function, characterized in that: The paper-based finishing material with anti-ultraviolet function is obtained by the preparation method described in any one of claims 1 to 9.
Citation Information
Patent Citations
Method for preparing antimicrobial material using nano calcium carbonate as substrate
CN101480194A
Highly-weather-resistant dip-dyed plain decorative base paper and preparation method thereof
CN108149511A
Ultraviolet-resistant sun-proof garment
CN109082882A
Preparation method and applications of calcium carbonate / titanium dioxide composite material
CN109181079A
Preparation method of paper-based packaging material with ultraviolet shielding function