Germanium-antimony-selenium-tellurium target metallographic display method

By using a mixed solution of potassium chlorate and sodium hydroxide as the corrosion solution, the safety risks and high cost of the metallographic display method of germanium, antimony, selenium tellurium target metallographic display method in the prior art are solved, and safety, environmental protection, low cost and corrosion uniformity are achieved. Metallographic display.

CN118961349APending Publication Date: 2024-11-15XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD

Patent Information

Application Number
CN202411293517.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The metallographic display method of the existing germanium antimony selenium tellurium target metallographic display uses strong acid corrosion agents, which has safety risks, high cost and difficult to control the corrosion effect. There is no report on the preparation method of metallographic sample for germanium antimony selenium tellurium tellurium target metallographic sample.

Method used

A mixed solution of potassium chlorate, sodium hydroxide and water is used as the corrosion solution, and metallographic samples are prepared through cutting, inlay, grinding and poking, avoiding the use of strong acid corrosion agents, and achieving safe, environmentally friendly and low-cost metallographic display.

Benefits of technology

It realizes the safety, environmental protection and low cost of metallographic display of germanium, antimony, selenium tellurium target metallographic display, good corrosion uniformity, clear surface display, simple operation, avoid the use of strong acid corrosion agents, and reduce safety risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118961349A_ABST
    Figure CN118961349A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of metallographic sample preparation, and discloses a germanium-antimony-selenium-tellurium target metallographic display method which comprises the following steps: cutting a germanium-antimony-selenium-tellurium target, mounting, roughly grinding, finely grinding, roughly polishing and finely polishing to obtain a germanium-antimony-selenium-tellurium target sample; the germanium-antimony-selenium-tellurium target material sample is subjected to metallographic corrosion in the corrosive liquid, and after cleaning and drying, a germanium-antimony-selenium-tellurium target material metallographic sample is obtained; the corrosive liquid is a mixed solution of potassium chlorate (KClO3), sodium hydroxide (NaOH) and water. The alkaline solution is used as the corrosive liquid, so that the use of a strong acid corrosive agent is avoided, particularly the use of a strong acid corrosive agent containing hydrofluoric acid is avoided, and the method is safe and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallographic sample preparation, and in particular relates to a method for metallographic display of germanium antimony selenium tellurium target materials. Background Art

[0002] Germanium antimony selenium telluride target is a phase change thin film material with the characteristics of high erasure rate, good thermal stability and cyclability, and low power consumption. It is the core material of phase change memory and has extremely broad application prospects. Generally, Germanium antimony selenium telluride thin films are prepared on substrates through powder metallurgy, hot pressing and magnetron sputtering. The performance of the film is not only affected by the purity, composition, oxygen content and density of the target material, but also has a close relationship with the internal structure such as grain size, morphology, uniformity, etc. Metallographic observation is the most direct and effective method to study the internal structure of the material.

[0003] Metallographic sample display methods generally include optical method, etching method, interference layer method, high temperature relief method, magnetic display method and decoration method. At present, the more commonly used method is etching method, which can be divided into electrolytic etching method, cathode vacuum etching method, thermal etching method, constant current etching method, etc. However, the above etching methods all require the use of equipment for etching, and the etching operation of metallographic samples is complicated and the cost is high. CN117347130A discloses a metallographic etching method and metallographic structure display method for germanium antimony tellurium alloy. The sample is prepared by cutting, rough grinding, fine grinding, polishing and other operations, and then a etching solution is prepared by using 40% hydrofluoric acid, 71% nitric acid and water in a ratio of 1:1:40, and the metallographic sample is obtained after cleaning and drying after etching for 10s to 20s.

[0004] CN115184124A discloses a metallographic etching method and metallographic structure display method for germanium telluride alloy. The sample is prepared by cutting, rough grinding, fine grinding, polishing and other operations, and then a etching solution is prepared by using 40% hydrofluoric acid, 36% to 38% hydrochloric acid, 65% to 68% nitric acid and water in a ratio of 2:3:5:10, and the metallographic sample is obtained after cleaning and drying after etching for 5s to 6s.

[0005] All of the above methods use hydrofluoric acid, which has a strong pungent odor and is extremely corrosive. It is highly dangerous and easily generates safety risks during use. In addition, there are problems such as the corrosion effect is difficult to control and the metallographic display is blurred. Moreover, there is currently no report on the metallographic sample preparation method for germanium antimony selenium tellurium target materials. Summary of the invention

[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method that is safe, environmentally friendly and suitable for metallographic display of germanium, antimony, selenium and tellurium targets.

[0007] To achieve the above objectives, the present invention provides the following specific technical solutions.

[0008] A method for metallographic display of germanium antimony selenium tellurium target material comprises the following steps: (1) After cutting, mounting, rough grinding, fine grinding, rough polishing and fine polishing, the germanium antimony selenium tellurium target material sample is obtained; (2) The germanium antimony selenium tellurium target material sample is subjected to metallographic etching in an etching solution, and after cleaning and drying, a metallographic sample of the germanium antimony selenium tellurium target material is obtained; The corrosive liquid is a mixed solution of potassium chlorate, sodium hydroxide and water.

[0009] In a further preferred embodiment, the mass ratio of potassium chlorate, sodium hydroxide and water is 3-6:1:10-20.

[0010] In a further preferred embodiment, the specific steps of the sample mounting are: placing the cut sample into a circular polyethylene mold, mixing epoxy resin and curing agent in a mass ratio of 7:3, pouring into the polyethylene mold, and solidifying.

[0011] In a further preferred embodiment, the coarse grinding, fine grinding, coarse polishing and fine polishing are carried out in an automatic grinding and polishing machine.

[0012] In a further preferred embodiment, the specific steps of the rough grinding are: using 100-500 mesh waterproof and wear-resistant silicon carbide sandpaper for grinding, the grinding speed is 250-350 r / min, and the grinding time is 15-40 min.

[0013] In a further preferred embodiment, the specific steps of fine grinding are: using 500-900 mesh sandpaper to fine grind the surface of the sample after rough grinding; the fine grinding speed is 250-350 r / min, and the fine grinding time is 15-40 min.

[0014] In a further preferred embodiment, the specific steps of the rough polishing are: using 1000-2000 mesh metallographic sandpaper to polish the surface of the sample after fine grinding, the polishing speed is 100-200 r / min, and the polishing time is 10-30 min.

[0015] In a further preferred embodiment, the specific steps of the fine polishing are: using a 0.1-6 μm polishing cloth and a 0.1-6 μm polishing spray for fine polishing, the fine polishing speed is 100-200 r / min, and the fine polishing time is 20-30 min.

[0016] Preferably, the polishing cloth is one of velvet polishing cloth, nylon polishing cloth, and porous chloroprene rubber, and more preferably is velvet polishing cloth.

[0017] Preferably, the polishing spray is one of silica polishing spray, alumina polishing spray, silicone polishing spray, and diamond polishing spray, and more preferably diamond polishing spray.

[0018] In a further preferred embodiment, after the fine polishing step, the surface of the germanium antimony selenium tellurium target material sample is cleaned with anhydrous ethanol.

[0019] In a further preferred embodiment, the corrosion time of the germanium antimony selenium tellurium target material sample in the etching solution is 30s~3min.

[0020] In a further preferred embodiment, after the etching is completed, the surface of the germanium antimony selenium tellurium target material sample is ultrasonically cleaned with pure water and anhydrous ethanol in sequence.

[0021] The surface of the germanium antimony selenium tellurium target sample after corrosion was observed through a metallographic microscope to obtain a metallographic image.

[0022] The above one or more technical solutions of the present invention can achieve at least one of the following beneficial technical effects: The invention adopts a mixed solution of potassium chlorate, sodium hydroxide and water as the etching liquid, thus avoiding the use of a strong acid etching agent, especially avoiding the use of a strong acid etching agent containing hydrofluoric acid, and has low cost, safety and environmental protection.

[0023] The present invention adopts potassium chlorate and sodium hydroxide as corrosion reagents, which can better control the corrosion rate and corrosion degree of the germanium antimony selenium tellurium target material, and the surface of the sample is corroded evenly.

[0024] The metallographic display method of germanium antimony selenium tellurium target material disclosed by the invention has simple operation and clear interface display. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a metallographic image of the sample surface after fine polishing obtained in step (2) of Example 1.

[0026] Figure 2 This is a metallographic image of the sample surface after corrosion in step (3) of Example 1.

[0027] Figure 3 This is a metallographic image of the sample surface after fine polishing obtained in step (2) of Example 2.

[0028] Figure 4 This is a metallographic image of the sample surface after corrosion in step (3) of Example 2.

[0029] Figure 5 This is a metallographic image of the sample surface after corrosion in step (3) of Example 3.

[0030] Figure 6 This is a metallographic image of the sample surface after corrosion in step (3) of Example 4.

[0031] Figure 7 This is a metallographic image of the sample surface after corrosion in step (3) of Example 5.

[0032] Figure 8 This is a metallographic image of the sample surface after corrosion in step (3) of Example 6. DETAILED DESCRIPTION

[0033] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0034] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0035] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0036] Example 1 The target material of germanium, antimony, selenium and tellurium with the composition content of 18% germanium, 29% antimony, 38% selenium and 15% tellurium was fixed on the electric spark cutting machine and cut into 15mm×10mm×5mm samples. The sample was placed in a circular polyethylene mold, and the epoxy resin and curing agent were prepared in a mass ratio of 7:3 and poured into the polyethylene mold. After solidification, the sample was taken out.

[0037] An automatic grinding and polishing machine was used to grind and polish the samples.

[0038] (1) Use 300-mesh waterproof and wear-resistant silicon carbide sandpaper to rotary grind the sample surface. The grinding speed is 350r / min and the grinding time is 20min, until there is no obvious machining trace on the polished surface. Then change to 800-mesh sandpaper to rotary fine grind the polished surface. The fine grinding speed is 350r / min and the fine grinding time is 20min.

[0039] (2) After fine grinding, use 1600 mesh metallographic sandpaper for polishing, the polishing speed is 200r / min, and the polishing time is 15min. After polishing, continue to use 0.3μm velvet polishing cloth with 0.3μm diamond polishing spray for fine polishing, the fine polishing speed is 200r / min, and the fine polishing time is 15min. Fine polishing until the surface is a bright mirror. After fine polishing, use anhydrous ethanol to clean the polishing agent and stains on the surface of the sample.

[0040] (3) Prepare a mixed solution of potassium chlorate, sodium hydroxide and water in a mass ratio of 3:1:20 and use it as a corrosion solution.

[0041] Place the sample on the corrosion platform, use a pipette to take an appropriate amount of corrosion liquid and drop it on the corrosion surface of the sample, and corrode for 1 minute. After the corrosion is completed, use pure water and anhydrous ethanol to perform ultrasonic cleaning for 5 minutes in turn. Then blow dry with a hair dryer, and then clean the metallographic display surface with wiping paper.

[0042] The metallographic sample surface of Germanium Antimony Selenium Telluride target was observed by metallographic microscope.

[0043] Figure 1 This is the metallographic image of the sample surface after fine polishing obtained in step (2). Figure 2 This is the metallographic image of the sample surface after corrosion in step (3). Figure 1 and Figure 2 After corrosion, a metallographic image with clear grain boundaries that is easy to identify is obtained.

[0044] Example 2 The target material of germanium, antimony, selenium and tellurium with the composition content of 16% germanium, 28% antimony, 39% selenium and 17% tellurium was fixed on the electric spark cutting machine and cut into 15mm×10mm×5mm samples. The sample was placed in a circular polyethylene mold, and the epoxy resin and curing agent were prepared in a mass ratio of 7:3 and poured into the polyethylene mold, and the sample was solidified and taken out.

[0045] An automatic grinding and polishing machine was used to grind and polish the samples.

[0046] (1) Use 400-mesh waterproof and wear-resistant silicon carbide sandpaper to perform rotary grinding on the metallographic surface. The grinding speed is 350r / min and the grinding time is 20min, so that there is no obvious machining trace on the polished surface. Then change to 900-mesh sandpaper for rotary fine grinding on the polished surface. The fine grinding speed is 350r / min and the fine grinding time is 20min.

[0047] (2) After fine grinding, use 1800 mesh metallographic sandpaper for polishing, the polishing speed is 200r / min, and the polishing time is 18min. After polishing, continue to use 0.1μm nylon polishing cloth and 0.1μm silica polishing spray for fine polishing, the fine polishing speed is 200r / min, and the fine polishing time is 18min. Fine polishing until the surface is a bright mirror. After fine polishing, use anhydrous ethanol to clean the polishing agent and stains on the surface of the sample.

[0048] (3) Prepare a mixed solution of potassium chlorate, sodium hydroxide and water in a mass ratio of 3:1:15 and use it as the etching solution. Place the sample on the etching platform, use a pipette to take an appropriate amount of etching solution and drop it on the etching surface of the sample, and etching for 50 seconds. After the etching is completed, ultrasonically clean it with pure water and anhydrous ethanol for 7 minutes in turn. Then blow it dry with a hair dryer, and then clean the metallographic display surface with wiping paper.

[0049] The metallographic sample surface of Germanium Antimony Selenium Telluride target was observed by metallographic microscope.

[0050] Figure 3 This is the metallographic image of the sample surface after fine polishing obtained in step (2). Figure 4 This is the metallographic image of the sample surface after corrosion in step (3). Figure 3 and Figure 4 After corrosion, a metallographic image with clear grain boundaries that is easy to identify is obtained.

[0051] Example 3 The target material of germanium, antimony, selenium and tellurium with the composition content of 20% germanium, 31% antimony, 36% selenium and 13% tellurium was fixed on the electric spark cutting machine and cut into 15mm×10mm×5mm samples. The sample was placed in a circular polyethylene mold, and the epoxy resin and curing agent were prepared in a mass ratio of 7:3 and poured into the polyethylene mold. After solidification, the sample was taken out.

[0052] An automatic grinding and polishing machine was used to grind and polish the samples.

[0053] (1) Use 500-mesh waterproof and wear-resistant silicon carbide sandpaper to rotary grind the metallographic surface. The grinding speed is 350r / min and the grinding time is 25min, until there is no obvious machining trace on the polished surface. Then change to 900-mesh sandpaper to rotary fine grind the polished surface. The fine grinding speed is 350r / min and the fine grinding time is 25min.

[0054] (2) After fine grinding, use 2000 mesh metallographic sandpaper for polishing, the polishing speed is 200r / min, and the polishing time is 15min. After polishing, continue to use 0.1μm velvet polishing cloth with 0.1μm alumina polishing spray for fine polishing, the fine polishing speed is 200r / min, and the fine polishing time is 15min. Fine polishing until the surface is a bright mirror. After fine polishing, use anhydrous ethanol to clean the polishing agent and stains on the surface of the sample.

[0055] (3) Prepare a mixed solution of potassium chlorate, sodium hydroxide and water in a mass ratio of 5:1:10 and use it as the etching solution. Place the sample on the etching platform, use a pipette to take an appropriate amount of etching solution and drop it on the etching surface of the sample, and etching for 35 seconds. After the etching is completed, ultrasonically clean it with pure water and anhydrous ethanol for 6 minutes in turn. Then blow it dry with a hair dryer, and then clean the metallographic display surface with wiping paper.

[0056] The metallographic sample surface of Germanium Antimony Selenium Telluride target was observed by metallographic microscope. Figure 5 This is a metallographic image of the sample surface after corrosion in step (3). It can be seen from the figure that the grain boundaries of the metallographic image are clear and easy to identify.

[0057] Example 4 The difference between Example 4 and Example 1 is that the etching liquid is a mixed solution of potassium chlorate, sodium hydroxide and water in a mass ratio of 4:1:18.

[0058] Figure 6 This is the metallographic display of the sample surface after corrosion in step (3).

[0059] Example 5 The difference between Example 5 and Example 1 is that the etching liquid is a mixed solution of potassium chlorate, sodium hydroxide and water in a mass ratio of 5:1:15.

[0060] Figure 7 This is the metallographic display of the sample surface after corrosion in step (3).

[0061] Example 6 The difference between Example 6 and Example 1 is that the etching liquid is a mixed solution of potassium chlorate, sodium hydroxide and water in a mass ratio of 3:1:40.

[0062] Figure 8 This is the metallographic display of the sample surface after corrosion in step (3).

[0063] from Figure 8 It can be seen that when the concentration of potassium chlorate and sodium hydroxide in the corrosion solution is too low, the corrosion effect is poor.

[0064] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for metallographic display of germanium antimony selenium tellurium target material, characterized in that: The following steps are involved: (1) After cutting, mounting, rough grinding, fine grinding, rough polishing and fine polishing, the germanium antimony selenium tellurium target material sample is obtained; (2) The germanium antimony selenium tellurium target material sample is subjected to metallographic etching in an etching solution, and after cleaning and drying, a metallographic sample of the germanium antimony selenium tellurium target material is obtained; The corrosive liquid is a mixed solution of potassium chlorate, sodium hydroxide and water.

2. The method for metallographic display of germanium antimony selenium tellurium target according to claim 1, characterized in that: The mass ratio of the potassium chlorate, sodium hydroxide and water is 3-6: 1: 10-20.

3. The method for metallographic display of germanium antimony selenium tellurium target material according to claim 1, characterized in that: The coarse grinding, fine grinding, coarse polishing and fine polishing are carried out in an automatic grinding and polishing machine.

4. The method for metallographic display of germanium antimony selenium tellurium target according to claim 1 or 3, characterized in that: The specific steps of the rough grinding are: using 100-500 mesh waterproof and wear-resistant silicon carbide sandpaper for grinding, the grinding speed is 250-350r / min, and the grinding time is 15-40min.

5. The method for metallographic display of germanium antimony selenium tellurium target according to claim 1 or 3, characterized in that: The specific steps of the fine grinding are: using 500-900 mesh sandpaper to fine grind the surface of the sample after rough grinding, the fine grinding speed is 250-350r / min, and the fine grinding time is 15-40min.

6. The method for metallographic display of germanium antimony selenium tellurium target according to claim 1 or 3, characterized in that: The specific steps of the rough polishing are: using 1000-2000 mesh metallographic sandpaper to polish the surface of the finely ground sample, the polishing speed is 100-200r / min, and the polishing time is 10-30min.

7. The method for metallographic display of germanium antimony selenium tellurium target according to claim 1 or 3, characterized in that: The specific steps of the fine polishing are: using a 0.1-6 μm polishing cloth and a 0.1-6 μm polishing spray for fine polishing, the fine polishing speed is 100-200 r / min, and the fine polishing time is 20-30 min.

8. The method for metallographic display of germanium antimony selenium tellurium target material according to claim 7, characterized in that: The polishing cloth is one of velvet polishing cloth, nylon polishing cloth, and porous chloroprene rubber; the polishing spray is one of silicon dioxide polishing spray, aluminum oxide polishing spray, silicone polishing spray, and diamond polishing spray.

9. The method for metallographic display of germanium antimony selenium tellurium target according to claim 1 or 2, characterized in that: The corrosion time of the Germanium Antimony Selenium Telluride target sample in the etching solution is 30s~3min.

10. The method for metallographic display of germanium antimony selenium tellurium target material according to claim 1, characterized in that: After the etching is completed, the surface of the germanium antimony selenium telluride target sample is ultrasonically cleaned with pure water and anhydrous ethanol in turn.

Citation Information

Patent Citations

  • Metallographic corrosion method and metallographic structure display method of germanium-antimony-tellurium alloy

    CN115184124A

  • Germanium telluride target metallographic display method

    CN117347130A

Cited By

  • Sample for electron back scattering diffraction analysis and preparation method thereof

    CN121090581A