Method for measuring content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method

Through pulse heating inert gas melting thermal conductivity method and combined with high-purity aluminum powder dilution technology, the problem of insufficient accuracy and range of aluminum nitride content detection in aluminum ash in the existing technology is solved, and the aluminum nitride content in aluminum ash is realized Efficient and accurate inspection, supporting efficient recycling and reuse of aluminum ash.

CN118961362APending Publication Date: 2024-11-15INST OF RES OF IRON & STEEL JIANGSU PROVINCE +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411071531.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing Kjeldahl nitrogen deposition method and the inert melting thermal conductivity method of oxygen nitrogen analyzer have problems such as cumbersome operation, long distillation time, large error and insufficient measurement range when detecting the aluminum nitride content in aluminum ash, resulting in poor detection accuracy. .

Method used

Using pulse heating inert gas melting thermal conductivity, a standard working curve is established by mixing reference aluminum nitride with high-purity aluminum powder to form an internally controlled dilution sample, and melting it in an oxygen-nitrogen hydrogen analyzer, and diluting it with high-purity aluminum powder. Test the aluminum ash sample to ensure the nitrogen content within the detection range, and calculate the aluminum nitride content in the aluminum ash to be tested.

Benefits of technology

It improves the accuracy and reliability of the detection of aluminum nitride content in aluminum ash, overcomes the problems of insufficient detection range and large errors, is simple and efficient in operation, accurate results, and is suitable for efficient recycling and reuse of aluminum ash.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118961362A_ABST
    Figure CN118961362A_ABST
Patent Text Reader

Abstract

The invention relates to the field of quantitative detection, and particularly discloses a method for determining the content of aluminum nitride in aluminum ash through a pulse heating inert gas melting thermal conductivity method. The method for determining the content of aluminum nitride in aluminum ash through the pulse heating inert gas melting thermal conductivity method comprises the following steps: mixing reference aluminum nitride and high-purity aluminum powder to form internal control dilution samples with different nitrogen element contents, analyzing the internal control dilution samples through an oxygen-nitrogen-hydrogen analyzer, and establishing a standard working curve; the method comprises the following steps: filling to-be-detected aluminum ash and high-purity aluminum powder into a nickel bag, putting the nickel bag into an oxygen-nitrogen-hydrogen analyzer for heating and melting, analyzing to obtain the nitrogen content WN in a mixed sample, and calculating to obtain the aluminum nitride content Wsample AlN in the to-be-detected aluminum ash. The method has the advantage of high accuracy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of quantitative detection, and more specifically, to a method for determining the content of aluminum nitride in aluminum ash by a pulse heating inert gas melting thermal conductivity method. Background Art

[0002] Aluminum will produce a large amount of solid waste with high aluminum content, namely aluminum ash, during the processing and production process. Aluminum ash mainly includes metallic aluminum, aluminum oxide, aluminum nitride and other components. Aluminum ash has economic value and great prospects for reuse due to its high content of metallic aluminum. The aluminum nitride content in aluminum ash is the key to the direction of aluminum ash recycling. Therefore, determining the aluminum nitride content in aluminum ash is of great significance for the recycling and reuse of aluminum ash.

[0003] In the related technology, the detection of nitrogen in high-temperature materials such as metals, metal alloys and ceramics mainly adopts the Kjeldahl method or the oxygen-nitrogen analyzer inert melt thermal conductivity method. However, the Kjeldahl method is cumbersome to operate and takes a long time to distill. There are problems such as long analysis cycle, difficult to control distillation time, and large errors caused by inapplicability of the method. The oxygen-nitrogen analyzer inert melt thermal conductivity method is more common in the detection of N in metal samples, but the instrument measurement range of the oxygen-nitrogen analyzer is 1×10 -7 -5×10 -3 However, the N content in general aluminum ash exceeds the measurement range of the instrument. Therefore, the accuracy of the measurement results of the oxygen-nitrogen analyzer inert molten thermal conductivity method in the detection of aluminum nitride content in aluminum ash is poor.

[0004] In view of the above-mentioned related technologies, the present invention further improves the inert melting thermal conductivity method of the oxygen-nitrogen analyzer, making the method suitable for detecting the aluminum nitride content in aluminum ash, thereby improving the accuracy and reliability of detecting the aluminum nitride content in aluminum ash. Summary of the invention

[0005] In order to improve the accuracy of the results of the detection of aluminum nitride content in aluminum ash, the present application provides a method for determining the aluminum nitride content in aluminum ash by pulse heating inert gas melting thermal conductivity method.

[0006] The method provided in the present application for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method adopts the following technical scheme:

[0007] A method for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method comprises the following steps:

[0008] The reference aluminum nitride and high-purity aluminum powder are mixed to form internal control dilution samples with different nitrogen content, and the internal control dilution samples with different nitrogen content are respectively loaded into nickel capsules, put into an oxygen, nitrogen and hydrogen analyzer to melt at 2100-2300°C, analyze the generated nitrogen, and establish a standard working curve with the ratio of the peak area to the mass of the aluminum ash internal control dilution sample as the horizontal coordinate and the nitrogen content of the aluminum ash internal control dilution sample as the vertical coordinate;

[0009] The aluminum ash to be tested and the high-purity aluminum powder are placed in a nickel capsule to obtain a nickel capsule coated with a mixed sample; the total mass of the mixed sample is 0.045-0.055 g, the mass of the aluminum ash to be tested is 0.002-0.01 g, and the mass of the high-purity aluminum powder is 0.043-0.045 g;

[0010] The nickel capsule coated with the mixed sample is put into an oxygen, nitrogen and hydrogen analyzer, heated and melted at 2100-2300℃, and the generated nitrogen is analyzed by the oxygen, nitrogen and hydrogen analyzer to obtain the nitrogen content W in the mixed sample. N , calculate the aluminum nitride content W in the aluminum ash to be tested 样AlN .

[0011] By adopting the above technical scheme, using high-purity aluminum powder as a diluent and nickel capsule as a flux, the aluminum nitride in the aluminum ash to be tested is reduced to generate nitrogen. By detecting the nitrogen content in the mixed sample, the aluminum nitride content in the aluminum ash to be tested is calculated.

[0012] This application uses high-purity aluminum powder as a diluent to reduce the nitrogen content of the mixed sample so that it is suitable for the detection range of the oxygen, nitrogen and hydrogen analyzer; the aluminum ash to be tested contains metallic aluminum. After dilution with high-purity aluminum powder, the types of components of the mixed sample do not change compared to the aluminum ash to be tested, and have no effect on the detection effect.

[0013] If the mass of the mixed sample is too large during the test, it is easy to burn incompletely and may exceed the capacity limit of the nickel capsule. If the mass of the mixed sample is too low, the weighing error will have a greater impact on the test result. Therefore, the mass of the mixed sample is limited to 0.045-0.055g; when the mass of the aluminum ash to be tested is less than 0.002g, the error fluctuation has a greater impact on the sample weight. When the mass of the aluminum ash to be tested is greater than 0.01g, a larger mass of high-purity aluminum powder is required to achieve a dilution effect, which may exceed the total mass limit of the mixed sample. Therefore, limiting the mass of the aluminum ash to be tested to 0.002-0.01g can achieve a better dilution effect for the mixed sample and reduce errors.

[0014] Preferably, the aluminum nitride content W 样AlN The calculation method of (%) is:

[0015] W 样AlN =W N ×A×(M rAlN / ArN ), A=(m 样 +m 纯铝 ) / m 样 ;

[0016] Where W N is the nitrogen content (%) in the aluminum ash and high-purity aluminum powder to be tested, m 样 is the mass of aluminum ash to be tested (g); m 纯铝 is the mass of high purity aluminum powder (g); M rAlN is the relative molecular mass of aluminum nitride; A rN is the relative atomic mass of nitrogen.

[0017] Preferably, by adjusting the analysis power, degassing power, purge time and comparator level parameters of the oxygen, nitrogen and hydrogen analyzer, the slope of the standard working curve is made to be 1±0.1 and the related linear coefficient is greater than 0.995.

[0018] Preferably, the analysis power of the oxygen, nitrogen and hydrogen analyzer is 5.0 kW, the degassing power is 5.8 kW, the purge time is 15 s, and the comparator level is 1.00%.

[0019] By adopting the above technical solution and the above analysis parameters, it is beneficial to further reduce the analysis error and improve the accuracy of the results.

[0020] Preferably, the internal control dilution sample is prepared on-the-fly and used immediately after preparation, and is prepared in a proportioned manner according to the required amount.

[0021] By adopting the above technical solution, the problem of non-representativeness of solid matter after being diluted is effectively avoided, which is conducive to making the standard working curve linear and accurate.

[0022] Preferably, the purity of the high-purity aluminum powder is ≥99.9%.

[0023] Preferably, the purity of the reference aluminum nitride is ≥99.9%.

[0024] Preferably, the particle size of the aluminum ash to be tested is 80-100 mesh.

[0025] Preferably, the method further comprises: mixing the aluminum ash to be tested with reference aluminum nitride, and performing a spiked recovery test.

[0026] Preferably, the spike recovery rate is 90-110%

[0027] Preferably, the oxygen, nitrogen and hydrogen analyzer measures nitrogen content using a pulse heating inert gas fusion-thermal conductivity detection method as the measurement principle.

[0028] In summary, this application has the following beneficial effects:

[0029] 1. This application achieves the effect of diluting the aluminum ash sample by adding high-purity aluminum powder, thereby overcoming the problem of low detection accuracy caused by the excessively high nitrogen content in the aluminum ash exceeding the detection range of the oxygen, nitrogen and hydrogen analyzer, and further ensures the detection accuracy by limiting the mass of the aluminum ash sample to be tested and the high-purity aluminum powder.

[0030] 2. This application adopts a proportional simulation method of high-purity metallic aluminum powder and reference aluminum nitride to simulate samples with different nitrogen contents according to the same processing steps to establish a working curve, and the internal control dilution sample adopts an instant preparation and on-demand preparation method, which reduces the possibility of inaccurate setting and is crucial to the establishment of instrument analysis conditions.

[0031] 3. The pulse heating inert gas melting-thermal conductivity method provided in this application for detecting the aluminum nitride content is simple and efficient to operate, has accurate results, is environmentally friendly, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is the standard working curve in the embodiment of this application. DETAILED DESCRIPTION

[0033] To further help understand the technical solution of the present invention, the technical solution of the present invention is described in more detail below by providing several specific implementation examples. All of these described embodiments are only partial embodiments of the present invention, not all of them.

[0034] The following specific embodiments may be combined with each other, and the same or similar concepts or processes may not be described in detail in some embodiments; and the reaction devices, monomer compounds, etc. involved in the following embodiments are all commercially available.

[0035] The following specific embodiments may be combined with each other, and the same or similar concepts or processes therein may not be described in detail in some embodiments.

[0036] The following examples are further explanations of the present invention, but the present invention is not limited thereto. Unless otherwise specified in the examples, the percentages are all by mass.

[0037] Example

[0038] This embodiment discloses a method for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method, comprising the following steps:

[0039] (1) Establishing a standard working curve

[0040] Referring to Table 1, the reference aluminum nitride and high-purity aluminum powder were mixed to form the following 5 groups of internal control dilution samples with different nitrogen content. In this embodiment, the reference aluminum nitride was purchased from Jinan Zhiding Welding Material Co., Ltd., and the high-purity aluminum powder was purchased from Shanghai Chemical Reagent Purchasing Co., Ltd.

[0041] Table 1

[0042]

[0043]

[0044] The five groups of internal control diluted samples were respectively loaded into nickel capsules and compacted, placed in a graphite crucible at the sampling port of an oxygen, nitrogen and hydrogen analyzer, melted at 2200°C, and the generated nitrogen was analyzed by the oxygen, nitrogen and hydrogen analyzer, the analysis power of the oxygen, nitrogen and hydrogen analyzer was 5.0kw, the degassing power was 5.8kw, the purge time was 15s, and the comparator level was 1.00%. In this embodiment, the model of the nickel capsule is LECOPART NO.502-822, and the model of the oxygen, nitrogen and hydrogen analyzer is LECO TCH600.

[0045] The ratio of the peak area to the mass of the aluminum ash internal control diluted sample is used as the horizontal axis, and the nitrogen content of the aluminum ash internal control diluted sample is used as the vertical axis to establish a standard working curve, such as Figure 1 The linear relationship of the standard working curve obtained by fitting is y=1.08763x+0.0021, and the correlation linear coefficient is 0.998.

[0046] (2) Precision detection of aluminum nitride content in aluminum ash to be tested

[0047] 2.1 Pass the aluminum ash sample through an 80-mesh sieve, weigh the sieve undersize and high-purity aluminum powder according to Table 2, and put them into a nickel bag for compaction;

[0048]

[0049]

[0050] 2.3 Place the nickel capsule containing the mixed sample in the graphite crucible of the oxygen, nitrogen and hydrogen analyzer inlet, melt it at 2200°C, keep the analysis power of the oxygen, nitrogen and hydrogen analyzer at 5.0kw, the degassing power at 5.8kw, the purge time at 15s, the comparator level at 1.00%, analyze the generated nitrogen by the oxygen, nitrogen and hydrogen analyzer, and obtain the nitrogen content determination value W in the mixed sample. N , according to W N铝灰 =W N ×A,A=(m 样 +m 纯铝 ) / m 样 , get the nitrogen content of the aluminum ash sample; according to W 样AlN =W N ×A×(M rAlN / A rN ), A=(m 样 +m 纯铝 ) / m 样 , and obtain the aluminum nitride content of the aluminum ash sample; where WN is the nitrogen content (%) in the aluminum ash and high-purity aluminum powder to be tested, m 样 is the mass of aluminum ash to be tested (g); m 纯铝 is the mass of high purity aluminum powder (g); M rAlN is the relative molecular mass of aluminum nitride; A rN is the relative atomic mass of nitrogen.

[0051] 2.4 The determination was performed seven times in parallel. The sample weight for each determination is shown in Table 2. The determination results are summarized in Table 3.

[0052] Table 3

[0053]

[0054] (3) Spike recovery test

[0055] Referring to Table 4, an aluminum ash sample with a nitrogen content of 4.11% was mixed with reference aluminum nitride and packed into a nickel bag for compaction. Referring to step 2.3, a spike recovery test was performed.

[0056] Table 4

[0057]

[0058] The spiked nitrogen content and the spiked recovery rate were obtained by analysis; the calculation method of the spiked nitrogen content and the recovery rate is as follows:

[0059] Added nitrogen content (g) = (m 基准AlN ×A rN ) / M rAlN ;

[0060] m 基准AlN is the mass of the base aluminum nitride (g), M rAlN is the relative molecular mass of aluminum nitride, A rN is the relative atomic mass of nitrogen;

[0061] Spiked recovery rate = ((m 总加标 ×W N加标 -m 铝灰 ×W N铝灰 ) / spike nitrogen content)×100;

[0062] m 总加标 W is the total mass of the spiked aluminum ash sample and the reference aluminum oxide. N加标 is the nitrogen content of the spiked sample obtained by oxygen, nitrogen and hydrogen analyzer, m 铝灰 is the mass of aluminum ash sample, W N铝灰 is the nitrogen content of the aluminum ash sample.

[0063] The determination was performed seven times in parallel. The sample weight for each determination is shown in Table 4. The determination results are summarized in Table 5.

[0064] Table 5

[0065]

[0066] Referring to Table 3, it can be seen that the detection precision reaches 1.21%. Referring to Table 5, it can be seen that the spike recovery rate of the aluminum ash sample is in the range of 93.8%-102.0%, which meets the requirements of the spike recovery test, indicating that the nitrogen content and aluminum nitride content in the aluminum ash sample are detected by referring to the method disclosed in this application. The test results are highly accurate and reliable, and meet daily analysis requirements.

[0067] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method, characterized in that: The following steps are involved: The reference aluminum nitride and high-purity aluminum powder are mixed to form internal control dilution samples with different nitrogen content, the internal control dilution samples with different nitrogen content are respectively loaded into nickel capsules, put into an oxygen, nitrogen and hydrogen analyzer to melt at 2100-2300° C., and the generated nitrogen is analyzed by the oxygen, nitrogen and hydrogen analyzer. The ratio of the peak area to the mass of the aluminum ash internal control dilution sample is used as the horizontal coordinate, and the nitrogen content of the aluminum ash internal control dilution sample is used as the vertical coordinate to establish a standard working curve; The aluminum ash to be tested and the high-purity aluminum powder are placed in a nickel capsule to obtain a nickel capsule coated with a mixed sample; the total mass of the mixed sample is 0.045-0.055 g, the mass of the aluminum ash to be tested is 0.002-0.01 g, and the mass of the high-purity aluminum powder is 0.043-0.045 g; The nickel capsule coated with the mixed sample is put into an oxygen, nitrogen and hydrogen analyzer, heated and melted at 2100-2300℃, and the generated nitrogen is analyzed by the oxygen, nitrogen and hydrogen analyzer to obtain the nitrogen content W in the mixed sample. N , calculate the aluminum nitride content W in the aluminum ash to be tested 样AlN .

2. The method for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method according to claim 1, characterized in that: The aluminum nitride content W 样AlN The calculation method of (%) is: W 样AlN =W N ×A×(M rAlN / A rN ),A=(m 样 +m 纯铝 ) / m 样 ; Where W N is the nitrogen content (%) in the aluminum ash and high-purity aluminum powder to be tested, m 样 is the mass of aluminum ash to be tested (g); m 纯铝 is the mass of high purity aluminum powder (g); M rAlN is the relative molecular mass of aluminum nitride; A rN is the relative atomic mass of nitrogen.

3. The method for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method according to claim 1, characterized in that: The slope of the standard working curve is 1±0.1, and the correlation linear coefficient is greater than 0.

995.

4. The method for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method according to claim 3, characterized in that: The analysis power of the oxygen, nitrogen and hydrogen analyzer is 5.0 kW, the degassing power is 5.8 kW, the purge time is 15 s, and the comparator level is 1.00%.

5. The method for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method according to claim 1, characterized in that: The internal control dilution sample is prepared in real time and used immediately after preparation, and is prepared in a proportion according to the required amount.

6. The method for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method according to claim 1, characterized in that: The purity of the high-purity aluminum powder is ≥99.9%; the purity of the reference aluminum nitride is ≥99.9%.

7. The method for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method according to claim 1, characterized in that: The particle size of the aluminum ash to be tested is 80-100 mesh.

8. The method for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method according to claim 1, characterized in that: Also includes: The aluminum ash to be tested is mixed with the reference aluminum nitride and a spike recovery test is carried out.

9. The method for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method according to claim 8, characterized in that: The spike recovery was 90-110%.

10. The method for determining the content of aluminum nitride in aluminum ash by pulse heating inert gas melting thermal conductivity method according to claim 1, characterized in that: The oxygen, nitrogen and hydrogen analyzer uses the pulse heating inert gas melting-thermal conductivity detection method as the measurement principle to measure the nitrogen content.