Nitrate ion selective electrode with ultralow detection lower limit
By using a combination of carboxylated polyvinyl chloride and anion exchange resin as internal filling in the nitrate ion selective electrode, the problems of short membrane life and high detection limit of traditional electrodes are solved, achieving higher sensitivity and stability.
Patent Information
- Application Number
- CN202411011105.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional nitrate-nitrogen ion selective electrodes suffer from problems such as short lifespan and high detection limit due to biomolecule adsorption and accumulation, and the concentration gradient of the internal filling solution affects the detection accuracy.
Carboxylated polyvinyl chloride is used as the electrode membrane skeleton structure, combined with anion exchange resin internal filling solution, to improve the hydrophilicity and stability of the electrode membrane and lower the detection limit.
It improves the hydrophilicity and lifespan of the electrode membrane, lowers the detection limit, enhances the sensitivity and stability of the electrode, reduces the adsorption of non-target substances, and improves the accuracy of measurement.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrochemical sensors, and in particular to a nitric nitrogen ion selective electrode with an ultra-low detection limit. Background Art
[0002] Nitrate ions are one of the common water and soil pollutants, and excessive release can pose risks to ecosystems and human health. In addition, in agricultural production, accurate measurement of nitrate concentrations in soil is also crucial for the management of rational fertilization of crops. Therefore, being able to accurately and quickly monitor nitrate ion concentrations in soil and water bodies and provide timely water quality information will help evaluate and control environmental pollution and improve crop production efficiency. Traditional nitrate detection methods including spectrophotometry, fluorescence and chemical analysis have limitations such as complex sample processing, long analysis time, sensitivity to interferences, dependence on laboratory equipment and high cost. In contrast, nitrate ion selective electrodes have the advantages of fast response, portability, high selectivity and low cost, making them a strong competitor in nitrate measurement.
[0003] Traditional nitrate-nitrogen ion selective electrodes have some drawbacks. The electrode membrane with PVC as the skeleton structure is a hydrophobic membrane, which tends to separate from the water phase, while biological molecules such as proteins and lipids are generally hydrophobic or amphiphilic. There is a mutual attraction between the hydrophobic surface of the electrode membrane and the hydrophobic region of the biological molecules, making it easy for the biological molecules to adsorb on the surface of the electrode membrane. During the online monitoring process of the electrode, the surface of the electrode membrane will face the adsorption and accumulation of protein and lipid biological substances. The accumulated biological substances will combine with the sensitive sites on the electrode membrane, reducing the selectivity of the electrode for the target ions; at the same time, the biofilm formed by the accumulated biological substances will introduce microorganisms, which will metabolize the components of the electrode membrane or produce chemical substances, damage the electrode membrane, and even cause the degradation of the electrode membrane, greatly reducing the service life of the electrode. In order to prevent the electrode from being disturbed by biological molecules during use and reducing its service life, CN 112557476A discloses an anti-oil polymer membrane ion selective electrode and its application, coating the electrode membrane surface with dopamine-polymethacrylate dimethyl propyl sulfonic acid ethyl ester coating, reducing the hydrophobic effect between the polymer sensitive membrane and the grease pollutants, preventing the adhesion of grease pollutants in water on the electrode membrane surface, and solving the grease problem faced by the polymer membrane potential type sensor when applied in complex water bodies. Although this method can improve the anti-fouling performance of the electrode membrane to a certain extent, it is necessary to add the step of surface modification of the electrode membrane, which increases the complexity of film making and the cost of the electrode membrane, and there is a risk of coating shedding during continuous use. In the prior art, some use doped PTFE powder to enter the electrode membrane, based on reducing the formation of the water layer between the membrane and the electrode (solid contact) and reducing the surface pollution of the sensor, to improve the long-term accuracy and durability of NO3-S-ISE for continuous wastewater monitoring. However, since PTFE particles are insoluble in this electrode membrane, how to make PTFE evenly dispersed in the electrode membrane is a great challenge.
[0004] Another drawback of traditional nitrate-nitrogen ion selective electrodes is that they are subject to the influence of the internal filling liquid, resulting in a less than ideal detection limit, which is generally only in the micromolar concentration range, severely limiting the electrode's ability to measure trace ions in environmental and clinical samples. The lower limit of detection is determined by the small amount of target ion flow that enters the aqueous surface of the organic sensor membrane. In nitrate-nitrogen ion selective electrodes, since the main ion concentration on the filling liquid side of the electrode membrane is generally higher than the ion concentration to be measured on the sample side, a certain concentration gradient is generated on both sides of the sensor membrane, which will cause the internal filling liquid to produce ion flow due to the concentration gradient during long-term use, resulting in the concentration of the sample ion detected by the sensor membrane to remain at a higher concentration. As a result, the concentration of the test solution is lower than 10 -6When the concentration of ions is 1.1777mol / L, this trace concentration added value that exists in the liquid membrane interface significantly affects the value of the membrane potential and severely limits the actual detection limit of the ion selective electrode. In order to improve the detection limit of the ion electrode, some scholars directly reduce the concentration of the target ion in the internal filling solution, but this has a certain impact on the long-term stability of the electrode, especially if the ion concentration in the internal filling solution is too different from that of the solution to be tested. Some scholars also use high-concentration interfering ions and low-concentration target ions as internal filling solutions, but high-concentration interfering ions may compete with target ions for active sites on the electrode surface, reducing the selectivity of the electrode for target ions. This may lead to a decrease in the accuracy of the measurement results. Some scholars have also introduced strong ion buffer systems such as complexing agents of the main ions into the internal filling solution to improve the detection limit of the electrode. However, as an anion, the nitrate ion has a relatively weak complexing ability and there is no suitable complexing agent to form a buffer system. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a nitrate-nitrogen ion selective electrode with an ultra-low detection limit, which uses special carboxylated polyvinyl chloride as a component of the skeleton structure of the electrode membrane to give the electrode membrane better hydrophilicity and reduce its detection limit.
[0007] (II) Technical solution
[0008] In order to achieve the above object, the main technical solutions adopted by the present invention include:
[0009] The invention provides a nitrate-nitrogen ion selective electrode with an ultra-low detection limit. The electrode is provided with an electrode membrane, and the electrode membrane is mainly made of the following components in parts by weight: 10 to 60 parts of carboxylated polyvinyl chloride, 0 to 60 parts of a plasticizer, 0.1 to 10 parts of a nitrate ion carrier, and 0 to 10 parts of an ion exchanger.
[0010] The present invention uses carboxylated polyvinyl chloride as the main component of the electrode membrane skeleton, which can improve the hydrophilicity of the electrode membrane, reduce the adsorption and accumulation of biological molecules such as proteins and lipids during the use of the electrode membrane, and improve the service life of the electrode. Carboxylated PVC is used as the skeleton structure of the electrode membrane. The carboxyl group (-COOH) introduced is a polar group, containing oxygen atoms and hydrogen bond donors (hydrogen atoms), and can form hydrogen bonds with hydrogen bond acceptors (oxygen atoms) in water molecules. At the same time, the introduction of carboxyl groups increases the active sites on the surface of the PVC material, and these sites can adsorb water molecules, resulting in the aggregation and diffusion of water molecules on the surface of the material, thereby improving the wettability of PVC and the adsorption capacity of water molecules. Therefore, without affecting the performance of the electrode, carboxylated PVC can effectively reduce the contact angle of the electrode membrane, improve the hydrophilicity of the electrode membrane, optimize the surface charge distribution of the membrane, repel some non-target hydrophobic (biological molecules) or neutral interfering substances, and improve the service life of the electrode. At the same time, the hydrophilicity of the electrode membrane surface is improved, making it easier for ions in the water phase to penetrate the membrane, improving the ion transmission efficiency and reducing interference, improving the sensitivity of the electrode, and further reducing the detection limit.
[0011] Optionally, the electrode membrane is mainly made of the following components in parts by weight: 10 to 60 parts of carboxylated polyvinyl chloride, 10 to 60 parts of plasticizer, 0.1 to 10 parts of nitrate ion carrier, and 0.1 to 10 parts of ion exchanger.
[0012] Optionally, in order to maintain a low detection limit for a long time, the present invention preferably has an average molecular weight of 100,000 to 500,000 for carboxylated polyvinyl chloride and a carboxylic acid content of 1 to 10%. Only within the above-defined range can the electrode have significantly optimal detection sensitivity and detection limit.
[0013] Optionally, the plasticizer is one or more of o-nitrophenyl octyl ether, dioctyl phthalate, dibutyl phthalate, diisobutyl phthalate, dioctyl adipate or dioctyl sebacate.
[0014] Optionally, the ion exchanger is one or a combination of two or more of tetraoctyl ammonium chloride, tridodecyl methyl ammonium chloride, trioctyl methyl ammonium chloride, and trihexyltetradecyl phosphonium chloride.
[0015] Optionally, the preparation method of the electrode membrane includes the following steps: dissolving carboxylated polyvinyl chloride, a plasticizer, an ion carrier, and an ion exchanger in a solvent, stirring for 1 to 2 hours, pouring the obtained mixed solution into a reactor, placing it horizontally, and drying to obtain a nitric nitrogen ion selective electrode membrane with a thickness of 0.1 to 0.8 mm.
[0016] Optionally, the electrode has an internal filling liquid, which is mainly composed of the following components in the following weight parts: 0.5-5 parts of nitrate, 90-95 parts of buffer solution, and 1-5 parts of anion exchange resin.
[0017] Adding anion exchange resin to the nitrate or potassium nitrate based filling solution to maintain a low constant concentration of the target ion is a complex forming agent. Anion exchange resins contain active groups, usually positively charged quaternary ammonium groups, which can release anions such as hydroxide ions or chloride ions. When nitrate ions flow through the resin, they will exchange ions with the active groups on the resin. The nitrate in the solution replaces the original hydroxide ions or chloride ions on the resin, and the OH- or Cl- released by the resin enters the solution. As the exchange continues, the active groups on the resin will gradually be saturated with anions in the solution. Once the resin reaches a saturated state, it can no longer adsorb anions in the solution. The concentration of the main ions in the filling solution is effectively reduced in the filling solution, resulting in a lower detection limit.
[0018] In addition, the inner filling liquid with anion exchange resin has a good match with the electrode membrane with carboxylated polyvinyl chloride. The hydrophilic property of the electrode membrane with carboxylated polyvinyl chloride can not only improve the sensitivity of the electrode membrane and reduce the detection limit, but also make up for the problem of decreased ion transmission efficiency caused by the inner filling liquid with anion exchange resin due to the lower detection limit. The two cooperate with each other to further dynamically adjust the concentration of nitrate ions in the inner filling liquid and effectively reduce the detection limit of the nitric nitrogen electrode membrane.
[0019] Optionally, the buffer solution is selected from one or more of potassium hydrogen phthalate-hydrochloric acid solution, potassium hydrogen phthalate-sodium hydroxide solution, sodium citrate solution, and sodium acetate-acetic acid solution with a pH of 6 to 7.
[0020] Optionally, the anion exchange resin is selected from one or more of a strongly basic anion exchange resin, a weakly basic anion exchange resin, and a mixed anion exchange resin.
[0021] Optionally, the method for preparing the internal filling solution comprises the following steps: dissolving nitrate in a buffer solution, stirring evenly, adding an anion exchange resin, and stirring for 6 to 8 hours to obtain the internal filling solution.
[0022] (III) Beneficial effects
[0023] The beneficial effects of the present invention are:
[0024] The ultra-low detection limit nitrate-nitrogen ion selective electrode provided by the present invention uses special carboxylated polyvinyl chloride as a component of the skeleton structure of the electrode membrane, which gives the electrode membrane good hydrophilicity and special binding sites, thereby reducing its detection limit. Furthermore, the present invention uses an anion exchange resin as a component of the internal filling liquid, which can cooperate with the electrode membrane to reduce the detection limit while ensuring the stability of the target ion concentration. DETAILED DESCRIPTION
[0025] In order to better explain the present invention, so as to facilitate understanding, exemplary embodiments of the present invention will be described in more detail below. It should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to be able to more clearly and thoroughly understand the present invention, and to be able to fully convey the scope of the present invention to those skilled in the art.
[0026] Example 1
[0027] This embodiment provides a nitric nitrogen ion selective electrode with an ultra-low detection limit, which comprises an electrode membrane and an internal filling liquid.
[0028] The preparation method of the electrode membrane is as follows: 100 mg of carboxylated polyvinyl chloride (carboxylic acid content 5%, molecular weight Mw = 100000), 200 mg of o-nitrophenyl octyl ether, 6 mg of nitrate carrier V, and 2 mg of tetraoctylammonium chloride are dissolved in 3 ml of anhydrous tetrahydrofuran, stirred for 1 hour, and the mixture is poured into a flat-bottomed glass container, placed horizontally, and naturally dried for 24 hours to obtain an ammonia nitrogen ion selective electrode membrane with a thickness of 0.3 mm. Finally, the membrane is cut into discs with a diameter of 10 mm using a punching tool and attached to the nitrate nitrogen ion selective electrode head containing the internal filling solution;
[0029] The preparation method of the internal filling liquid is as follows: dissolve 1g of sodium nitrate in 100ml of potassium hydrogen phthalate-hydrochloric acid buffer solution with a pH of 6.8, stir evenly, add 3g of strongly basic anion exchange resin, and stir with a mechanical stirrer for 6-8h to obtain the internal filling liquid.
[0030] Example 2
[0031] This embodiment provides a nitric nitrogen ion selective electrode with an ultra-low detection limit, which comprises an electrode membrane and an internal filling liquid.
[0032] The preparation method of the electrode membrane is as follows: 100 mg of carboxylated polyvinyl chloride (carboxylic acid content 1%, molecular weight Mw = 100000), 150 mg of ethylene glycol phthalate, 6 mg of nitrate carrier V, 2 mg of trihexyltetradecylphosphonium chloride are dissolved in 1.5 ml of anhydrous tetrahydrofuran, stirred for 1 hour, until the sensitive membrane mixed solution is formed, and then the mixture is poured into a flat-bottomed glass container, placed horizontally, and naturally dried for 24 hours to obtain a nitrate-nitrogen ion selective electrode membrane with a thickness of 0.5 mm. Finally, the membrane is cut into discs with a diameter of about 10 mm using a punching tool and attached to the nitrate-nitrogen ion selective electrode head containing the internal filling solution.
[0033] The preparation method of the internal filling liquid is as follows: the internal filling liquid is 0.8g of sodium nitrate dissolved in 100ml of sodium acetate-acetic acid buffer solution with a pH of 6.8, after stirring evenly, 2g of weakly alkaline anion exchange resin is added, and the internal filling liquid is obtained by stirring with a mechanical stirrer for 6h.
[0034] Example 3
[0035] This embodiment provides a nitric nitrogen ion selective electrode with an ultra-low detection limit, which comprises an electrode membrane and an internal filling liquid.
[0036] The preparation method of the electrode membrane is as follows: 600 mg of carboxylated polyvinyl chloride (carboxylic acid content 1-10%, molecular weight 500000), 100 mg of dioctyl phthalate, 1 mg of nitrate carrier V, 100 mg of tridodecyl methyl ammonium chloride are dissolved in 3 ml of anhydrous tetrahydrofuran, stirred for 1-2 hours, the obtained mixed solution is poured into a flat-bottomed glass container, placed horizontally, and naturally dried for 24 hours to obtain an ammonia nitrogen ion selective electrode membrane with a thickness of 0.3 mm. Finally, the membrane is cut into discs with a diameter of 10 mm using a punching tool and attached to the nitric nitrogen ion selective electrode head containing the internal filling solution;
[0037] The preparation method of the internal filling solution is as follows: dissolve 0.5 g of sodium nitrate in 100 ml of potassium hydrogen phthalate-hydrochloric acid buffer solution with a pH of 6.8, stir evenly, add 1 g of mixed anion exchange resin, and stir with a mechanical stirrer for 8 hours to obtain the internal filling solution.
[0038] Example 4
[0039] This embodiment provides a nitric nitrogen ion selective electrode with an ultra-low detection limit, which comprises an electrode membrane and an internal filling liquid.
[0040] The preparation method of the electrode membrane is as follows: 300 mg of carboxylated polyvinyl chloride (carboxylic acid content 1-10%, molecular weight 100000), 300 mg of diisobutyl phthalate, 10 mg of nitrate carrier V, 20 mg of trihexyltetradecylphosphonium chloride are dissolved in 3 ml of anhydrous tetrahydrofuran, stirred for 1-2 hours, the obtained mixed solution is poured into a flat-bottomed glass container, placed horizontally, and naturally dried for 24 hours to obtain an ammonia nitrogen ion selective electrode membrane with a thickness of 0.3 mm. Finally, the membrane is cut into discs with a diameter of 10 mm using a punching tool and attached to the nitrate nitrogen ion selective electrode head containing the internal filling solution;
[0041] The preparation method of the internal filling liquid is as follows: dissolve 5g of sodium nitrate in 95ml of potassium hydrogen phthalate-hydrochloric acid buffer solution with a pH of 6.8, stir evenly, add 5g of weakly basic anion exchange resin, and stir with a mechanical stirrer for 6h to obtain the internal filling liquid.
[0042] Comparative Example 1
[0043] This comparative example provides a nitrate-nitrogen ion selective electrode with an ultra-low detection limit, and the steps are the same as those of Example 1, except that carboxylated polyvinyl chloride is replaced by polyvinyl chloride.
[0044] Comparative Example 2
[0045] This comparative example provides a method for preparing an ammonia nitrogen ion selective electrode membrane, and the steps are the same as those of Example 1, except that the potassium hydrogen phthalate-hydrochloric acid buffer solution with a pH of 6.8 is replaced by deionized water.
[0046] Comparative Example 3
[0047] This comparative example provides a method for preparing an ammonia nitrogen ion selective electrode membrane, and the steps are the same as those of Example 1, except that no anion exchange resin is added.
[0048] Comparative Example 4
[0049] This comparative example provides a method for preparing an ammonia nitrogen ion selective electrode membrane, and the steps are the same as those of Example 1, except that carboxylated polyvinyl chloride with a carboxylic acid content of 15% is used.
[0050] Comparative Example 5
[0051] This comparative example provides a method for preparing an ammonia nitrogen ion selective electrode membrane, and the steps are the same as those of Example 1, except that carboxylated polyvinyl chloride with a carboxylic acid content of 0.1% is used.
[0052] Comparative Example 6
[0053] This comparative example provides a method for preparing an ammonia nitrogen ion selective electrode membrane, and the steps are the same as those of Example 1, except that half of the carboxylated polyvinyl chloride is replaced by polyvinyl chloride.
[0054] Comparative Example 7
[0055] This comparative example provides a method for preparing an ammonia nitrogen ion selective electrode membrane, and the steps are the same as those of Example 1, except that half of the carboxylated polyvinyl chloride is replaced with polyvinyl chloride, and no anion exchange resin is added.
[0056] The electrodes prepared in Example 1 and Comparative Examples 1-7 were used to measure the performance parameters of the nitric ion selective electrode membrane, such as contact angle, detection limit, slope, response time and service life, as shown in the following table.
[0057] Among them, the determination method of slope, response range and detection limit is:
[0058] Contact angle measurement method: Use a contact angle measuring instrument, such as a contact angle meter or a contact angle measuring instrument, and perform measurements according to standard operating procedures. Place the nitrate-nitrogen ion selective electrode membrane on the test instrument, drop water onto the membrane surface, and record the contact angle when the water drop contacts the membrane surface.
[0059] Method for determining the lower limit of detection: gradually dilute the nitric nitrogen standard solution, observe the changes in the electrode output signal, and determine the lowest nitric nitrogen concentration that can be stably detected.
[0060] Slope determination method: Use standard nitric acid solution to prepare standard solutions of different concentrations, measure the relationship between the output potential and the logarithmic concentration, and calculate the slope value.
[0061] Response time determination method: Within a certain concentration range, quickly change the nitric nitrogen concentration, record the change of electrode output potential over time, and calculate the response time by curve fitting.
[0062] Service life determination method: Conduct long-term stability tests, record changes in electrode output signals over time, and evaluate electrode performance degradation.
[0063] The contact angle of the electrode membrane is used to evaluate the hydrophilicity of the membrane surface. The lower the contact angle, the better the hydrophilicity. The detection limit of the electrode ensures the lowest nitrate concentration that can be detected. The slope of the electrode reflects the sensitivity and performance of the electrode. Ideally, according to the Nernst equation, the slope of the electrode should be 59.16mV / dec at 25°C. In fact, due to the characteristics of the electrode membrane, temperature fluctuations, ionic strength and other factors, the actual slope may deviate from the theoretical value, and the general value is 59±3mV / dec. The response time refers to the time required for the electrode to reach 95% of the stable value from the beginning of contact with the sample to the output potential. It reflects the reaction speed of the electrode to the change of ion concentration and is an important indicator of the dynamic performance of the electrode. Improving the service life of the electrode can reduce the frequency of electrode maintenance and replacement required by users, simplify the operation process, improve work efficiency, reduce maintenance costs, and improve economic benefits.
[0064]
[0065] From the above table, it can be seen that the electrode made of carboxylated polyvinyl chloride in the present invention has a significantly lower contact angle and a longer service life than polyvinyl chloride. In particular, the carboxyl content in carboxylated polyvinyl chloride must be between 1% and 10%. Too high a content or too low a content does not help the service life. A high content of carboxylic acid makes the electrode membrane have better hydrophilicity, but it cannot increase the service life and reduce the detection limit, indicating that the contribution of carboxylated polyvinyl chloride is not only its hydrophilicity.
[0066] When the amount of carboxylated polyvinyl chloride added is reduced to half, the values of various parameters decrease. From the data of Comparative Example 1, Comparative Example 3, Comparative Example 6 and Comparative Example 7, it can be seen that the carboxylated polyvinyl chloride and the anion exchange resin must cooperate with each other, and have a positive contribution to the contact angle, service life, detection limit, etc.
[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An ultra-low detection limit nitrate-nitrogen ion selective electrode, the electrode is provided with an electrode membrane, characterized in that: The electrode membrane is mainly made of the following components in parts by weight: 10 to 60 parts of carboxylated polyvinyl chloride, 0 to 60 parts of plasticizer, 0.1 to 10 parts of nitrate ion carrier, and 0 to 10 parts of ion exchanger.
2. The ultra-low detection limit nitrate-nitrogen ion selective electrode according to claim 1, characterized in that: The electrode membrane is mainly made of the following components in parts by weight: 10 to 60 parts of carboxylated polyvinyl chloride, 10 to 60 parts of plasticizer, 0.1 to 10 parts of nitrate ion carrier, and 0.1 to 10 parts of ion exchanger.
3. The ultra-low detection limit nitrate-nitrogen ion selective electrode according to claim 1, characterized in that: The average molecular weight of the carboxylated polyvinyl chloride is 100,000 to 500,000, and the carboxylic acid content is 1 to 10%.
4. The ultra-low detection limit nitric nitrogen ion selective electrode according to claim 1, characterized in that: The plasticizer is one or a combination of two or more of o-nitrophenyl octyl ether, dioctyl phthalate, dibutyl phthalate, diisobutyl phthalate, dioctyl adipate or dioctyl sebacate.
5. The ultra-low detection limit nitrate-nitrogen ion selective electrode according to claim 1, characterized in that: The ion exchanger is one or a combination of two or more of tetraoctyl ammonium chloride, tridodecyl methyl ammonium chloride, trioctyl methyl ammonium chloride, and trihexyltetradecyl phosphonium chloride.
6. The ultra-low detection limit nitrate-nitrogen ion selective electrode according to claim 1, characterized in that: The preparation method of the electrode membrane comprises the following steps: dissolving carboxylated polyvinyl chloride, a plasticizer, a nitrate ion carrier and an ion exchanger in a solvent, stirring for 1 to 2 hours, pouring the obtained mixed solution into a reactor, placing it horizontally, and drying to obtain a nitrate-nitrogen ion selective electrode membrane with a thickness of 0.1 to 0.8 mm.
7. The ultra-low detection limit nitrate-nitrogen ion selective electrode according to any one of claims 1 to 6, characterized in that: The electrode has an internal filling liquid, which is mainly prepared by the following components in the following weight parts: 0.5 to 5 parts of nitrate, 90 to 95 parts of buffer solution, and 1 to 5 parts of anion exchange resin.
8. The ultra-low detection limit nitrate-nitrogen ion selective electrode according to claim 7, characterized in that: The buffer solution is one or a combination of two or more of potassium hydrogen phthalate-hydrochloric acid solution, potassium hydrogen phthalate-sodium hydroxide solution, sodium citrate solution, and sodium acetate-acetic acid solution with a pH between 6 and 7.
9. The ultra-low detection limit nitrate-nitrogen ion selective electrode according to claim 7, characterized in that: The anion exchange resin is one of a strongly basic anion exchange resin, a weakly basic anion exchange resin, and a mixed anion exchange resin, or a combination of two or more thereof.
10. The ultra-low detection limit nitrate-nitrogen ion selective electrode according to claim 7, characterized in that: The preparation method of the internal filling solution comprises the following steps: dissolving nitrate in a buffer solution, stirring evenly, adding anion exchange resin, and stirring for more than 6 hours to obtain the internal filling solution.