Method for processing light-splitting and beam-combining cemented prism

Through the processing method of spectroscopic beam glued prism, photosensitive adhesives and precision measurement tools are used to eliminate double aberrations, improve the image quality and discrimination rate of glued prisms, solve the problems of insufficient double aberration and accuracy in the existing technology, and realize the Efficient optical processing.

CN118962938APending Publication Date: 2024-11-15HENAN PINGYUAN OPTO ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411021754.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the spectrosynthetic beam glued prism has double aberration problems during processing, resulting in poor image quality and insufficient discrimination accuracy, which limits the mass production of products.

Method used

A method of photosynthesis beam glued prism processing, including glueing and precuring the prism with photosensitive adhesive, followed by full curing, fine grinding and polishing to ensure the plane optical properties of the glued prism, and adjusting the light through a goniometer to eliminate it Double aberration and grinding and cylindrical processing under specific environmental conditions ensure high accuracy of the parts.

Benefits of technology

It effectively solves the double aberration problem, improves the image quality and discrimination accuracy of the spectrosynthetic beam glued prism, simplifies the processing process, reduces the processing difficulty, and ensures the high accuracy and stability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118962938A_ABST
    Figure CN118962938A_ABST
Patent Text Reader

Abstract

The invention relates to a method for processing a light-splitting and beam-combining cemented prism in the field of optical processing. The method comprises the following steps: S1, preparing a qualified prism I and a qualified prism II for manufacturing the cemented prism; s2, gluing and pre-curing the prism I and the prism II by using a photosensitive adhesive; s3, fully curing the glued prism I and prism II; s4, the first face of the cemented prism is fixed through optical cement, and accurate grinding and polishing are conducted on the second face of the cemented prism; s5, the second face of the cemented prism is fixed through optical cement, and accurate grinding and polishing are conducted on the first face of the cemented prism; s6, clamping and positioning the glued prism of which the two surfaces are polished, and grinding the outer circle of the third surface of the glued prism; and S7, after the glued prism subjected to outer circle grinding processing is detected to be qualified, the next process is turned to. The invention aims to solve the problem of double aberration of the light-splitting and beam-combining cemented prism processed in the prior art, so that the image quality is good, and meanwhile, the discrimination rate reaches relatively high precision.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optical processing, and in particular relates to a method for processing a light-splitting, beam-combining and glued prism. Background Art

[0002] The beam splitter and beam combiner is made of a beam splitter right angle prism and a common right angle prism glued together to split and transmit multiple beams. In some cases, the beam splitter prism can be combined into a single component, such as combining two 45° right angle prisms into a 90° beam splitter prism. Such a combination can reduce the number of reflections and the required space, while improving the stability and efficiency of the system.

[0003] In recent years, beam splitter and beam combiner prisms are increasingly used in the military industry, such as optical lenses, etc. The process is difficult, especially the double aberration and identification rate problems restrict the mass production needs of products. How to effectively solve the double aberration problem of beam splitter and beam combiner prisms and achieve a high precision in the identification rate of parts has always been a technical problem that plagues the optical processing field of beam splitter and beam combiner prisms. Summary of the invention

[0004] In view of the above situation, the present invention provides a method for processing a beam-splitting and beam-combining glued prism, which aims to solve the double aberration problem existing in the beam-splitting and beam-combining glued prism processed in the prior art, so as to improve the image quality and achieve a higher identification rate accuracy.

[0005] In order to achieve the above purpose, the present invention adopts the following technical solutions:

[0006] A method for processing a light-splitting and beam-combining glued prism comprises the following steps:

[0007] S1. Prepare qualified prism 1 and prism 2 for making cemented prism;

[0008] S2, using photosensitive adhesive to glue and pre-cure prism 1 and prism 2;

[0009] S3, fully curing the glued prism 1 and prism 2;

[0010] S4, fixing the first surface of the bonded prism with light glue, and fine grinding and polishing the second surface of the bonded prism;

[0011] S5, fix the second surface of the glued prism with light glue, and finely grind and polish the first surface of the glued prism; S6, clamp and position the glued prism after polishing on both sides, and grind the outer circle of the third surface of the glued prism; S7, after the outer circle grinding, the glued prism is tested and passed and then transferred to the next process.

[0012] Furthermore, the process indicators for judging whether prism 1 and prism 2 are qualified in step S1 include: prism 1 and prism 2 must be processed using the same piece of strip material to ensure that the refractive index of the two prisms is the same, avoid the optical path deflection of the outgoing light due to slight differences in the refractive index, and ensure the smooth progress of the subsequent gluing process; prism 1 and prism 2 are both optical prisms with a right-angled trapezoidal longitudinal section, one base angle of the right-angled trapezoid is 45°, the angle accuracy is ≤7″, and the actual measured value of the 45° angle is measured and marked with a goniometer; the absolute value of the difference between the actual measured values ​​of the 45° angle of prism 1 and prism 2 is <5″.

[0013] like Figure 1 As shown, the distance from the center point O of the glued prism to the third surface is L, the thickness is d, and the diameter is D. Because the first and second surfaces of the glued prism need to be polished after gluing, it is necessary to reserve a processing allowance of 0.4mm for the upper and lower surfaces of prism one, and a processing allowance of 0.5mm for the upper and lower surfaces of prism two. The trapezoidal bottom edge of prism one needs to reserve a processing allowance of 0.5mm for the edge grinding process.

[0014] The length of the base of the trapezoid of prism 1

[0015] L′=D-L+(d+0.8)÷2+0.5mm;

[0016] The formula for calculating the chord height of prism 2 is:

[0017]

[0018] The tolerance is -0.2mm; Figure 3 As shown, the width of prism 1 and prism 2 is D+2 mm, where 2 mm is the edge grinding allowance in the side width direction.

[0019] Since the first and second surfaces of the glued prisms 1 and 2 are processed to flatten the protruding parts and have a good surface shape, the accuracy of the part identification rate is guaranteed; the edge grinding process ensures that the dimensional accuracy of the parts meets the requirements through the use of a special edge grinding joint.

[0020] Furthermore, in step S2, a photosensitive adhesive of model NOA61 (which is more sensitive to ultraviolet light with a wavelength of 350 to 380 nm) is used to glue the right-angled trapezoidal surface of prism one and the right-angled trapezoidal surface of prism two. The preferred environmental requirements of the gluing workshop are: temperature 18°C ​​to 26°C, humidity 30% to 70%; at the same time, under the goniometer, it is adjusted so that the three cross images formed by the incident light entering from the first surface of the glued prism and the outgoing light emitted from its second and third surfaces overlap, and no double image exists.

[0021] like Figure 1As shown in the figure, the cemented prism, the single prism 2 of which is a beam splitter, the light is incident along the SM direction, and is split into two beams at point O, namely OM and OP, among which the incident beam SO, the outgoing beam OM and OP, all three beams show a cross image on the goniometer reticle pattern, as shown Figure 2 When the three cross images overlap, there is no double aberration in the SM direction of the cemented prism and the image quality is good. On the contrary, there is double aberration in the SM direction of the cemented prism.

[0022] Then use ultraviolet light or 100W mercury lamp to irradiate the prism for 5 minutes at a distance of 5 to 10cm to pre-cure the photosensitive adhesive; after gluing prism 1 and prism 2, make sure that the first surface of prism 2 is 0.2mm higher than the first surface of prism 1, and the second surface of prism 2 is flush with that of prism 1; that is, the thickness of prism 2 is 0.2mm greater than that of prism 1. Figure 3 and 4 shown.

[0023] Furthermore, in step S3, the pre-cured glued prism is placed at room temperature for 24 hours before being cured, and then irradiated with light again for 2 hours in a UV oven, and then placed at room temperature for 48 hours to fully cure the photosensitive adhesive, and then transferred to the polishing process.

[0024] Furthermore, in step S4, the cured first surface of the bonded prism is fixed on the pad to form a mirror plate, and then the second surface of the bonded prism is finely ground and polished using a polishing machine; the second surface of the bonded prism is finely ground to a thickness of 0.5 mm, so that the second surface of the bonded prism is completely finely ground, and the parallelism of the mirror plate is required to be controlled within 0.001 mm; the second surface of the bonded prism after polishing is controlled to have a surface shape of N=0.5 and ΔN=0.2; the parallelism between the first surface and the second surface of the bonded prism is ≤5″, and after passing the self-inspection, it is transferred to the next step.

[0025] The optimal environmental requirements for the photoresist workshop are: temperature 22℃~24℃.

[0026] The requirements for the preferred optical adhesive pad are: surface shape N≤0.5, ΔN≤0.2, one side can be polished, and the thickness difference measured with a micrometer is ≤0.001mm.

[0027] Furthermore, in step S5, the glued prism is turned over so that the second surface of the glue is fixed on the pad to form a mirror plate, and then the first surface of the glued prism is finely ground and polished using a polishing machine; the first surface of the glued prism is finely ground to a thickness of 0.5 mm, and the second surface of the glued prism is completely finely ground to require that the parallelism of the mirror plate is controlled to be 0.001 mm; after polishing, the second surface of the glued prism is controlled to have a surface shape of N=0.5 and ΔN=0.2; the parallelism between the first surface and the second surface of the glued prism is ≤5″, and after passing the self-inspection, the outer circle grinding process is performed.

[0028] like Figure 4As shown, after prism 1 and prism 2 are glued together, a 1.6-meter parallel light tube and a 40x front mirror are used to observe the discrimination plate in the direction of the optical axis SM, and good image quality and no double images are used as the self-inspection pass standard.

[0029] The gluing process adjusts the coincidence of three images under the goniometer, that is, the coincidence of the three cross images of the incident light SO, the outgoing light OM and the OP light beam on the goniometer. This is the first key point in the prism gluing process; it ensures that the image quality of the parts in the SM direction is good after gluing and there is no double image.

[0030] During the polishing process, the parallelism difference between the first and second surfaces of the glued prism is controlled twice to be ≤5″. This is the second key point in the prism gluing process. It maintains the coincidence of the three images in the SM direction, which indirectly ensures that the image quality of the polished part in the SM direction is good and there is no double image.

[0031] Furthermore, in step S6, the polished first and second surfaces of the bonded prism are clamped and positioned using a dedicated edge grinding joint 1 and edge grinding joint 2, and then the third surface of the bonded prism is subjected to an outer circle grinding (also called edge grinding) process.

[0032] like Figure 5 As shown, when the glued prism is positioned, the auxiliary sheet can be used to ensure that the third surface of the glued prism is flush with the platform surface on one side of the edge grinding joint 2, so as to ensure the distance from its center point O to its third surface. Then the auxiliary sheet can be removed and the edge grinding machine can be used for edge grinding. After the edge grinding is completed, the dihedral angle is chamfered, and after passing the inspection, it is transferred to the next process.

[0033] like Figure 6 As shown, the entire process of manufacturing the glued prism is: prepare qualified prisms 1 and 2 → glue → cure with ultraviolet oven → gloss glue the first surface → fine grind and polish the second surface → gloss glue the second surface → fine grind and polish the first surface → grind the outer circle → transfer to the next process.

[0034] The glued prism parts processed by this processing method have no double images and good image quality when inspecting the parts from the SM direction; at the same time, the identification rate of the parts can reach 8" when inspecting the parts within the range of φ30mm.

[0035] The present invention also includes other components that enable it to be used normally, all of which are conventional means in the field. In addition, devices or components not limited in the present invention, such as: ultraviolet oven, photoresist pad, edge grinding joint, polishing machine, edge grinding machine, auxiliary sheet, etc., all adopt the existing technology in the field.

[0036] The beneficial effects of the present invention are as follows:

[0037] The present invention provides a method for processing a beam-splitting and beam-combining glued prism, which uses polishing equipment, an ultraviolet oven, an Abbe goniometer, a precision goniometer and other detection tools, operating specifications and process parameters such as polishing and gluing, and stipulates corresponding process quality control. The glued prism processing method ensures that the indicators of the beam-splitting and beam-combining glued prism meet the requirements through a simple process flow and control of relevant process parameters, is simple and easy to operate, has strong operability, and a short processing time. It can effectively control the processing accuracy of the beam-splitting and beam-combining prism, effectively improve the processing accuracy of the beam-splitting and beam-combining glued prism, ensure that the image quality of the beam-splitting and beam-combining glued prism in the SM direction is good and there is no double image, and at the same time, the parts identification rate meets the requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 The figure is a schematic diagram of the overall structure of a glued prism formed by gluing prism 1 and prism 2 in the present invention.

[0039] Figure 2 It is a schematic diagram of imaging on the goniometer when observing along the SM direction during the gluing process in the present invention.

[0040] Figure 3 Schematic diagram of the technical requirements for preparing the individual pieces of prism 1 and prism 2 before the gluing process in the present invention.

[0041] Figure 4 The figure is a schematic diagram of the positional relationship between prism 1 and prism 2 during the gluing process and the gluing process in the present invention.

[0042] Figure 5 It is a schematic diagram of grinding the outer circle to the center in the edging process after gluing, curing and polishing in the present invention.

[0043] Figure 6 The figure is an overall process flow chart of the method for processing the photosplitting and beam combining glued prism in the present invention.

[0044] Figure 7 Schematic diagram of the overall structure of a glued prism formed by gluing prism 1 and prism 2 in the embodiment.

[0045] Figure 8 Schematic diagram of the technical requirements for preparing the individual pieces of prism 1 and prism 2 before the gluing process in the embodiment.

[0046] Fig. 9 Schematic diagram of the positional relationship between prism 1 and prism 2 during the gluing process and the gluing process in the embodiment.

[0047] Fig.10 It is a schematic diagram of the structure and size of edge grinding joint 1 and edge grinding joint 2 in the edge grinding process in the embodiment. DETAILED DESCRIPTION

[0048] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments.

[0049] Example

[0050] like Figure 7 As shown, the technical requirements of the beam splitter and combiner prism to be processed are: observation with a 1.6-meter collimator and a 40x front mirror in the direction of the optical axis SM, a discrimination rate of 8″, good image quality, and no double image.

[0051] The method for processing a light-splitting beam-combining glued prism comprises the following steps:

[0052] S1, preparing qualified prism 1 and prism 2 for making cemented prism 10;

[0053] S2, using photosensitive adhesive to glue and pre-cure the prism 1 101 and the prism 2 102;

[0054] S3, fully curing the glued prism 1 and prism 2;

[0055] S4, fix the first surface 1001 of the glued prism with optical glue, and finely grind and polish the second surface 1002 of the glued prism;

[0056] S5, fix the second surface 1002 of the glued prism with optical glue, and finely grind and polish the first surface 1001 of the glued prism;

[0057] S6, clamping and positioning the glued prism after polishing on both sides, and grinding the outer circle of the third surface 1003 of the glued prism;

[0058] S7. After the outer circle grinding process, the glued prism is tested and qualified and then transferred to the next process.

[0059] Specifically, in step S1, qualified prism 1 and prism 2 are prepared, such as Figure 7 As shown, the distance from the center point O of the cemented prism to the three faces is 19.4-0.1mm, the thickness is 13-0.2mm, and the diameter of the part is φ41mm;

[0060] The length of the base of the prism is

[0061] L′=D-L+(d+0.8)÷2+0.5=41-19.4+(13+0.8)÷2+0.5=29mm,

[0062] The chord height of prism 2 is

[0063]

[0064] The tolerance is -0.2mm; the side width of prism 1 and prism 2 is

[0065] D+2=41+2=43mm.

[0066] Adding other indicators, the technical requirements of Prism 1 and Prism 2 are formed, such as Figure 8 shown.

[0067] It should be noted that:

[0068] 1) Use Prismmaster precision goniometer to measure the 45° angle values ​​of prism 1 and prism 2;

[0069] 2) The surface shape is N = 0.5, ΔN = 0.2, which is slightly stricter to ensure the accuracy of the prism angle value;

[0070] 3) Prism 1 and prism 2 must be produced from the same piece of material to ensure that the refractive index of the two single pieces of material is the same.

[0071] Specifically, in step S2, before the gluing process, the selection is made: the absolute value of the difference between the measured values ​​of the 45° angle of prism one and prism two is required to be less than 5″, and then the gluing can begin.

[0072] like Fig. 9 As shown, during the gluing process, a photosensitive adhesive of model NOA61 (which is more sensitive to ultraviolet light with a wavelength of 350-380nm) is used to glue the right-angled trapezoidal bevel 1014 of prism one and the right-angled trapezoidal bevel 1024 of prism two. Under the model JJC2S Abbe goniometer, it is adjusted to the overlap of three images (the three cross images of the incident light SO, the outgoing light OM and the OP light beam on the goniometer overlap, and there is no double image). Then, an ultraviolet lamp or a 100-watt mercury lamp is used to irradiate the parts at a distance of 5-10cm for 5 minutes for pre-curing, and then the parts are placed at room temperature for 24 hours for curing.

[0073] Specifically, in step S3, UVGO ultraviolet oven is selected for curing for 2 hours (its working wavelength is 365nm), and then it is placed at room temperature for 48 hours before switching to the polishing process.

[0074] Specifically, in step S4, firstly, the second surface of the cemented prism is finely ground and polished, and the specific steps are as follows:

[0075] S41, first side of optical glue: glue the first side of the prism onto the backing plate to form a mirror plate;

[0076] S42, fine grinding and polishing the second surface: fine grinding the second surface to a size of 0.5 mm below, so that the second surface is completely fine ground, and the parallelism of the mirror plate is controlled to 0.001 mm; polishing the second surface, controlling the surface shape: N = 0.5, ΔN = 0.2;

[0077] S43, Self-check parallelism: Self-check the parallelism difference between the first and second surfaces of the glued prism is ≤5″. After passing the inspection, proceed to the next step.

[0078] Specifically, in step S5, the first surface of the cemented prism is turned over and finely ground and polished. The specific steps are as follows:

[0079] S51, optical glue second side: glue the optical glue of the second side of the prism onto the backing plate to form a mirror plate;

[0080] S52, fine grinding and polishing the first surface: fine grinding the first surface to a size of 0.5 mm below the first surface, so that the first surface is completely fine ground, and the parallelism of the mirror plate is controlled to 0.001 mm; polishing the first surface, controlling the surface shape: N = 0.5, ΔN = 0.2;

[0081] S53, Self-check parallelism error: Self-check the parallelism error between the first and second surfaces of the glued prism is ≤5″. After passing the inspection, proceed to the external grinding process.

[0082] It should be noted that the polished surface shapes N=0.5 and ΔN=0.2 of the first and second surfaces of the glued prism need to be strictly controlled to ensure the identification accuracy of the glued prism.

[0083] Specifically, in step S6, a special edge grinding joint 1 20 and an edge grinding joint 2 30 are used in the process of grinding the outer circle, such as Fig.10 As shown, the dimension from the axis of the second edge grinding joint to the joint platform is 19.4-0.03-0.07. Before machining the part, use the auxiliary sheet 40 to adjust the part position so that the platform surface of the second edge grinding joint is flush with the third surface of the glued prism. When grinding the outer circle, remove the auxiliary sheet first, and then start grinding the outer circle of the third surface of the glued prism. In order to ensure the requirement of 19.4-0.1 for the part, the part position needs to be adjusted during the edge grinding process. Please refer to Figure 5 Then chamfer the dihedral angle according to the drawing requirements, and after passing the inspection, it can be transferred to the next process.

[0084] It should be noted that during the processing, the environmental requirements of the gluing workshop are: temperature 18℃~26℃, humidity 30%~70%; the environmental temperature and humidity are related to the quality of prism gluing and photo-gluing process, affecting the angular value accuracy and surface defects of parts, which is very important for high-precision optical parts processing;

[0085] The absolute value of the difference between the measured values ​​of the 45° angle of the selected prism 1 and prism 2 is less than 5″; Environmental requirements for the photosensitive adhesive workshop: temperature 22℃~24℃; The selection of the 45° measured values ​​of prism 1 and prism 2 ensures a more uniform photosensitive adhesive layer during the gluing process;

[0086] The pad is made of φ220~φ300 optical adhesive pad, with surface shape: N≤0.5, ΔN≤0.2, and one side is polished. The thickness difference measured by micrometer is ≤0.001mm; the optical adhesive pad is the basic tooling for processing optical parts, and its surface shape and thickness difference indirectly affect the parallel error control of the processed glued prism.

[0087] The present invention is mainly applicable to the processing of light-splitting beam-combining glued prisms, and can also improve the processing accuracy of such prisms and greatly reduce their processing difficulty. The technical solution of the present invention is not limited to the above-mentioned specific embodiments. Without departing from the scope and spirit of the described embodiments, many modifications and changes are obvious to ordinary technicians in this technical field. Any technical deformation made within the spirit and principle of the present invention falls within the protection scope of the present invention.

Claims

1. A method for processing a light-splitting and beam-combining prism, characterized in that: The following steps are involved: S1. Prepare qualified prism 1 and prism 2 for making cemented prism; S2, using photosensitive adhesive to glue and pre-cure prism 1 and prism 2; S3, fully curing the glued prism 1 and prism 2; S4, fixing the first surface of the bonded prism with light glue, and fine grinding and polishing the second surface of the bonded prism; S5, fixing the second surface of the bonded prism with light glue, and fine grinding and polishing the first surface of the bonded prism; S6, clamping and positioning the glued prism after polishing on both sides, and grinding the outer circle of the third side of the glued prism; S7. After the outer circle grinding process, the glued prism is tested and qualified and then transferred to the next process.

2. The method for processing a beam splitting and combining prism according to claim 1, characterized in that: The process indicators for judging whether prism 1 and prism 2 are qualified in step S1 include: prism 1 and prism 2 must be processed using the same piece of strip material to ensure that the refractive index of the two prisms is the same; prism 1 and prism 2 are both optical prisms with a right-angle trapezoidal longitudinal section, and one base angle of the right-angle trapezoid is 45°, the angle accuracy is ≤7″, and the actual measured value of the 45° angle is measured and marked with a goniometer; the absolute value of the difference between the actual measured values ​​of the 45° angle of prism 1 and prism 2 is <5″.

3. The method for processing a beam splitting and combining prism according to claim 1, characterized in that: In step S2, the right-angled trapezoidal bevel of prism one and the right-angled trapezoidal bevel of prism two are glued together using photosensitive adhesive, and at the same time, the three cross images formed by the incident light entering from the first surface of the glued prism and the outgoing light emitted from the second and third surfaces thereof are adjusted under a goniometer so that the three cross images are completely overlapped, so that the glued prism has no double aberration, and at the same time, light irradiation is used to pre-cure the photosensitive adhesive.

4. The method for processing a light-splitting and beam-combining glued prism according to claim 3, characterized in that: The photosensitive adhesive used in step S2 is NOA61 photosensitive adhesive, which is pre-cured by irradiating the prism with ultraviolet light or a 100-watt mercury lamp for 5 minutes at a distance of 5 to 10 cm from the prism. After the photosensitive adhesive of the bonding prism is pre-cured, ensure that the first surface of prism two is higher than the first surface of prism one, and then leave it at room temperature for 24 hours before curing.

5. The method for processing a beam splitting and combining prism according to claim 1, characterized in that: In step S3, the pre-cured glued prism is irradiated with light again to fully cure the photosensitive adhesive. The pre-cured glued prism that has been left at room temperature for 24 hours is placed in a UV oven for further curing for 2 hours, and then left at room temperature for 48 hours to fully cure the photosensitive adhesive.

6. The method for processing a light-splitting and beam-combining glued prism according to claim 1, characterized in that: In step S4, the cured first surface of the bonded prism is fixed on the backing plate to form a mirror plate, and then the second surface of the bonded prism is finely ground and polished; after polishing, the second surface of the bonded prism is controlled to have a surface shape of N=0.5 and ΔN=0.2; and the parallelism between the first surface and the second surface of the bonded prism is ≤5″.

7. The method for processing a light-splitting and beam-combining glued prism according to claim 6, characterized in that: In step S5, the glued prism is turned over so that the second surface of the glue is fixed on the pad to form a mirror plate, and then the first surface of the glued prism is finely ground and polished; after polishing, the second surface of the glued prism is controlled to have a surface shape of N=0.5 and ΔN=0.2; and the parallelism between the first surface and the second surface of the glued prism is ≤5″.

8. A method for processing a light-splitting and beam-combining glued prism according to claim 6 or 7, characterized in that: The pad is required to be a smooth plastic pad with a surface shape of N≤0.5 and ΔN≤0.

2. The pad can be polished on one side, and the thickness difference between the two surfaces at different positions must be ≤0.001mm.

9. The method for processing a beam splitting and combining prism according to claim 1, characterized in that: In step S6, the first and second surfaces of the bonded prism after polishing are clamped and positioned using edge grinding joints 1 and 2, and then the third surface of the bonded prism is subjected to outer circle grinding. When positioning the bonded prism, ensure that the third surface of the bonded prism is flush with one side of the edge grinding joint 2.